Specific Process Knowledge/Etch/ICP Metal Etcher/silicon/nano/Sinano4: Difference between revisions
Appearance
Created page with "== The Sinano4.0 recipe == {| border="2" cellpadding="2" cellspacing="1" |+ '''Recipe Sinano4.0''' |- ! rowspan="6" align="center"| Recipe | Gas | Cl<sub>2</sub> 20 sccm |- ..." |
|||
| Line 1: | Line 1: | ||
== The Sinano4.0 recipe == | == The Sinano4.0 recipe == | ||
<!-- revised 1/6-2015 by jmli --> | |||
{| border="2" cellpadding="2" cellspacing="1" | {| border="2" cellpadding="2" cellspacing="1" | ||
|+ '''Recipe Sinano4.0''' | |+ '''Recipe Sinano4.0''' | ||
Revision as of 13:12, 1 June 2015
The Sinano4.0 recipe
| Recipe | Gas | Cl2 20 sccm |
|---|---|---|
| Pressure | 2 mTorr, Strike 3 secs @ 5 mTorr | |
| Power | 900 W CP, 60 W PP | |
| Temperature | 20 degs | |
| Hardware | 100 mm Spacers | |
| Time | 90 secs | |
| Conditions | Run ID | 435, ID |
| Conditioning | Sequence: Oxygen clean, MU tests, processes, no oxygen between runs | |
| Mask | 110 nm zep etched down to 43 nm |
- The results of the Sinano4.0 recipe
-
The 30 nm trenches
-
The 60 nm trenches
-
The 90 nm trenches
-
The 120 nm trenches
-
The 150 nm trenches
| Nominal trench line width | ' | ' | 30 | 60 | 90 | 120 | 150 | Average | Std. dev. |
| Etch rate | nm/min | 154 | 169 | 170 | 172 | 177 | 169 | 9 | |
| Sidewall angle | degs | 85 | 83 | 84 | 84 | 84 | 84 | 1 | |
| CD loss | nm/edge | 28 | 52 | 68 | 87 | 101 | 67 | 29 | |
| CD loss foot | nm/edge | 28 | 52 | 68 | 87 | 101 | 67 | 29 | |
| Bowing | 24 | 28 | 24 | 20 | 16 | 22 | 5 | ||
| Bottom curvature | -21 | 18 | 20 | 15 | 11 | 9 | 17 | ||
| Zep etch rate | 45 |