Jump to content

Specific Process Knowledge/Lithography/Aligners/MAvsMLA: Difference between revisions

Taran (talk | contribs)
Taran (talk | contribs)
Line 19: Line 19:
==AZ 5214E==
==AZ 5214E==
===Resolution===
===Resolution===
'''Resolution at optimal conditions for different exposure equipment:'''
'''Resolution at optimal processing conditions for different exposure equipment:'''
{| class="wikitable"
{| class="wikitable"
|+
|+
Line 113: Line 113:


===Yield===
===Yield===
The yield is measured by inspecting all 116 lithographic resolution test structures in an optical microscope and recording the smallest resolved dots and lines.
The yield is measured by inspecting all 116 lithographic resolution test structures in an optical microscope and recording the smallest resolved dots and lines.
<br clear="all" />
<br clear="all" />
Line 188: Line 189:


===Resist profile===
===Resist profile===
====Linewidth and sidewall angle vs exposure dose====
====Linewidth and sidewall angle vs exposure dose====
'''SEM images of 2µm triplets as a function of exposure dose:'''
'''SEM images of 2µm triplets as a function of exposure dose:'''
{|border="1" cellspacing="0" cellpadding="3" style="text-align:left;"  
{|border="1" cellspacing="0" cellpadding="3" style="text-align:left;"  
Line 214: Line 217:


|}
|}
 
<br clear="all" />


{|border="1" cellspacing="0" cellpadding="3" style="text-align:left;"  
{|border="1" cellspacing="0" cellpadding="3" style="text-align:left;"  
Line 238: Line 241:


|}
|}
 
<br clear="all" />


'''Result of image analysis of SEM images of 2µm triplets:'''
'''Result of image analysis of SEM images of 2µm triplets:'''
Line 245: Line 248:
! width="510" |   
! width="510" |   


|+'''Width of 2µm line and sidewall angle vs. exposure dose for 1.5µm AZ 5214E.'''
|+
|- border="0" align="center"
|- border="0" align="center"
|[[Image:5214E_Linewidth vs dose.jpg|500px]]
|[[Image:5214E_Linewidth vs dose.jpg|500px]]
Line 251: Line 254:


|- align="center"
|- align="center"
| colspan="2" | Blue circles: Exposed on Aligner: MA6-2 in vacuum contact. <br>Orange Squares: Exposed on Aligner: Maskless 02 (MLA2) using defoc 2 (QC defoc=2).   
| colspan="2" | Width of 2µm line and sidewall angle vs. exposure dose for 1.5µm AZ 5214E. <br>Blue circles: Exposed on Aligner: MA6-2 in vacuum contact. <br>Orange Squares: Exposed on Aligner: Maskless 02 (MLA2) using defoc 2 (QC defoc=2).   
|}
|}
<br clear="all" />
<br clear="all" />


====Linewidth and sidewall angle vs defocus parameter====


====Linewidth and sidewall angle vs defocus parameter====
'''SEM images as a function of defocus parameter for Aligner: Maskless 02 (MLA2) using dose 95mJ/cm<sup>2</sup>:'''
'''SEM images as a function of defocus parameter for Aligner: Maskless 02 (MLA2) using dose 95mJ/cm<sup>2</sup>:'''
{|border="1" cellspacing="0" cellpadding="3" style="text-align:left;"  
{|border="1" cellspacing="0" cellpadding="3" style="text-align:left;"  
Line 290: Line 293:


|}
|}
 
<br clear="all" />


'''Result of image analysis of SEM images of 2µm triplets:'''
'''Result of image analysis of SEM images of 2µm triplets:'''
Line 296: Line 299:
! width="510" |  
! width="510" |  


|+'''Linewidth and sidewall angle vs. defocus value  for 1.5µm AZ 5214E exposed in Aligner: Maskless 02 (MLA2) using dose 95mJ/cm<sup>2</sup>.'''
|+
|- border="0" align="center"
|- border="0" align="center"
|[[Image:5214E_Profile vs defoc.jpg|500px]]
|[[Image:5214E_Profile vs defoc.jpg|500px]]


|- align="center"
|- align="center"
| Blue circles: Width of 2µm line. <br>Orange Squares: Sidewall angle.
| Linewidth and sidewall angle vs. defocus value  for 1.5µm AZ 5214E exposed in Aligner: Maskless 02 (MLA2) using dose 95mJ/cm<sup>2</sup>. <br>Blue circles: Width of 2µm line. <br>Orange Squares: Sidewall angle.


|}
|}