Specific Process Knowledge/Lithography/Aligners/MAvsMLA: Difference between revisions
| Line 187: | Line 187: | ||
===Resist profile (linewidth and sidewall angle)=== | ===Resist profile (linewidth and sidewall angle)=== | ||
'''SEM images of 2µm triplets as a function of exposure dose:''' | '''SEM images of 2µm triplets as a function of exposure dose:''' | ||
{|border="1" cellspacing="0" cellpadding="3" style="text-align:left;" | {|border="1" cellspacing="0" cellpadding="3" style="text-align:left;" | ||
| Line 212: | Line 213: | ||
|} | |} | ||
{|border="1" cellspacing="0" cellpadding="3" style="text-align:left;" | {|border="1" cellspacing="0" cellpadding="3" style="text-align:left;" | ||
| Line 235: | Line 237: | ||
|} | |} | ||
'''Result of image analysis of SEM images of 2µm triplets:''' | '''Result of image analysis of SEM images of 2µm triplets:''' | ||
| Line 250: | Line 253: | ||
|} | |} | ||
<br clear="all" /> | <br clear="all" /> | ||
'''SEM images as a function of defocus parameter for Aligner: Maskless 02 (MLA2):''' | |||
{|border="1" cellspacing="0" cellpadding="3" style="text-align:left;" | |||
|- | |||
|- | |||
|-style="background:silver; color:black" | |||
! | |||
!Defoc -8 | |||
!Defoc -1 | |||
!Defoc 2 | |||
!Defoc 5 | |||
!Defoc 12 | |||
|- | |||
|- | |||
|-style="background:WhiteSmoke; color:black" | |||
|2µm triplets | |||
|[[Image:W14 MA62 5214E vac D85_H6B_01.jpg|280px]] | |||
|[[Image:W14 MA62 5214E vac D90_H4B_01.jpg|280px]] | |||
|[[Image:W14 MA62 5214E vac D95_F3B_01.jpg|280px]] | |||
|[[Image:W14 MA62 5214E vac D100_B4T_01.jpg|280px]] | |||
|[[Image:W14 MA62 5214E vac D105_C6T_01.jpg|280px]] | |||
|- | |||
|-style="background:WhiteSmoke; color:black" | |||
|Lines | |||
|[[Image:W14 MA62 5214E vac D85_H6B_01.jpg|280px]] | |||
|[[Image:W14 MA62 5214E vac D90_H4B_01.jpg|280px]] | |||
|[[Image:W14 MA62 5214E vac D95_F3B_01.jpg|280px]] | |||
|[[Image:W14 MA62 5214E vac D100_B4T_01.jpg|280px]] | |||
|[[Image:W14 MA62 5214E vac D105_C6T_01.jpg|280px]] | |||
|} | |||
{| cellpadding="2" style="border: 2px solid darkgray;" align="left" | {| cellpadding="2" style="border: 2px solid darkgray;" align="left" | ||
| Line 260: | Line 299: | ||
|- align="center" | |- align="center" | ||
| Blue circles: Width of 2µm line. <br>Orange Squares: Sidewall angle. | | Blue circles: Width of 2µm line. <br>Orange Squares: Sidewall angle. | ||
|} | |} | ||
<br clear="all" /> | <br clear="all" /> | ||
Revision as of 13:57, 15 June 2026
The content on this page, including all images and pictures, was created by DTU Nanolab staff, unless otherwise stated.
Feedback to this page: click here
Mask Aligner vs Maskless Aligner
Slides presented at NNUM in Uppsala 2026: MA6 vs MLA 2026_v09
Mask design used in the investigation: LithoTestAlign_2025_v10.gds
Additional data
THIS PAGE IS UNDER CONSTRUCTION
AZ 5214E
Resolution
| Exposure equipment | Dose | Contact/Defoc | Resolution | Comment |
|---|---|---|---|---|
| Aligner: MA6-2 | 100 | Vacuum | 1µm | |
| Aligner: MA6-1 | 100 | Vacuum | 1.25µm | Probably over-exposed |
| Aligner: Maskless 02 (MLA2) | 90 | 2 | 1.25µm |
SEM images from different exposure equipment:
| 2µm triplets | Lines | Trenches | |
|---|---|---|---|
| Aligner: MA6-2
100mJ/cm2, vacuum contact |
|||
| Aligner: MA6-1
100mJ/cm2, vacuum contact |
|||
| Aligner: Maskless 02 (MLA2)
90mJ/cm2, defoc 2 |
SEM images of different size structures:
| 1µm triplets | 2µm triplets | 4µm triplets | |
|---|---|---|---|
| Aligner: MA6-1
100mJ/cm2, vacuum contact |
Yield
The yield is measured by inspecting all 116 lithographic resolution test structures in an optical microscope and recording the smallest resolved dots and lines.
Effect of exposure mode for mask aligner
Effect of WEC pressure for mask aligner (after WEC head service)
Resist profile (linewidth and sidewall angle)
SEM images of 2µm triplets as a function of exposure dose:
| 85mJ/cm2 | 90mJ/cm2 | 95mJ/cm2 | 100mJ/cm2 | 105mJ/cm2 | |
|---|---|---|---|---|---|
| Aligner: MA6-2
Vacuum contact |
| 80mJ/cm2 | 90mJ/cm2 | 100mJ/cm2 | 110mJ/cm2 | |
|---|---|---|---|---|
| Aligner: Maskless 02 (MLA2)
Defoc 2 |
Result of image analysis of SEM images of 2µm triplets:
SEM images as a function of defocus parameter for Aligner: Maskless 02 (MLA2):
| Defoc -8 | Defoc -1 | Defoc 2 | Defoc 5 | Defoc 12 | |
|---|---|---|---|---|---|
| 2µm triplets | |||||
| Lines |
| Blue circles: Width of 2µm line. Orange Squares: Sidewall angle. |
AZ MiR 701
Resolution
- Table with optimal parameters and resolution for different aligners
- SEM pictures
Resist profile (sidewall angle and linewidth)
- SEM pictures to support graphs?

Blue circles: Exposed on Aligner: MA6-2 in vacuum contact.
Orange Squares: Exposed on Aligner: Maskless 02 (MLA2) using defoc 2 (QC defoc=2).

Blue circles: Exposed on Aligner: MA6-2 in vacuum contact.
Orange Squares: Exposed on Aligner: Maskless 02 (MLA2) using defoc 2 (QC defoc=2).

Blue circles: Width of 2µm line. Orange Squares: Sidewall angle.
AZ nLOF 2020
Resolution
- Table with optimal parameters and resolution for different aligners
- SEM pictures
Resist profile (sidewall angle and linewidth)
- SEM pictures to support graphs?

Blue circles: Exposed on Aligner: MA6-2 in vacuum contact.
Orange Squares: Exposed on Aligner: Maskless 01 (MLA1) using defoc -4 (QC defoc=-2).
Grey triangles: Exposed on Aligner: Maskless 02 (MLA2) using defoc 0 (QC defoc=2).

Blue circles: Exposed on Aligner: MA6-2 in vacuum contact.
Orange Squares: Exposed on Aligner: Maskless 01 (MLA1) using defoc -4 (QC defoc=-2).
Grey triangles: Exposed on Aligner: Maskless 02 (MLA2) using defoc 0 (QC defoc=2).

Blue circles: Width of 2µm line. Orange Squares: Sidewall angle.

Blue circles: Width of 2µm line. Orange Squares: Sidewall angle.