Specific Process Knowledge/Lithography/Descum: Difference between revisions
| Line 200: | Line 200: | ||
[[File:PA_descum_multi_v3.png|400px|thumb|Ashing amount and ashing rate when processing multiple 100 mm wafers. Test measured on the center of 3 wafers.|right]] | [[File:PA_descum_multi_v3.png|400px|thumb|Ashing amount and ashing rate when processing multiple 100 mm wafers. Test measured on the center of 3 wafers.|right]] | ||
{| class="wikitable" style="caption-side: top; text-align: | {| class="wikitable" style="text-align: center;" | ||
|+ style="caption-side: top; text-align: left;" | Ashing amount and rate | |||
|- | |- | ||
! style="text-align: left;" | Ashing time [min]: !! 1 !! 2 !! 5 !! 10 !! 15 | ! style="text-align: left;" | Ashing time [min]: !! 1 !! 2 !! 5 !! 10 !! 15 | ||
| Line 209: | Line 210: | ||
|} | |} | ||
{| class="wikitable" style="caption-side: top; text-align: | {| class="wikitable" style="text-align: center;" | ||
|+ style="caption-side: top; text-align: left;" | Ashing non-uniformity | |||
|- | |- | ||
! style="text-align: left;" | Ashing time [min]: !! 1 !! 2 !! 5 !! 10 !! 15 | ! style="text-align: left;" | Ashing time [min]: !! 1 !! 2 !! 5 !! 10 !! 15 | ||
Revision as of 17:09, 26 February 2025
The content on this page, including all images and pictures, was created by DTU Nanolab staff, unless otherwise stated.
Feedback to this page: click here
Plasma Asher 1
Plasma asher 1 was decommissioned 2024-12-02.
Information about decommissioned tool can be found here.
Plasma Asher 2
Plasma asher 2 was decommissioned 2024-12-02.
Information about decommissioned tool can be found here.
Plasma Asher 3: Descum
The user manual(s), quality control procedure(s) and results and contact information can be found in LabManager - requires login
Plasma Asher 3 is specifically used for controlled descum process after lithography. Please note that you only can process a single 100 mm wafer, or one small sample, at a time. The plasma asher is equipped with 2 gaslines: oxygen and nitrogen, but all standard processes use only oxygen (as recommended by Diener).
Ashing of AZ MiR701 resist:
You can use two different descum process developments: you can either change power settings or processing chamber pressure.
Testing different power settings:

Recipe settings:
- O2 flow: 5 sccm
- N2 flow: 0
- Pressure: 0.2 mbar
- Power: Varied
Experiment parameters:
|
Testing different pressure settings:

Recipe settings:
- O2 flow: varied
- N2 flow: 0
- Pressure: varied
- Power: V100% (100 W)
Experiment parameters:
|
Ashing of AZ5214E resist:

Recipe settings:
- O2 flow: varied
- N2 flow: 0
- Pressure: varied
- Power: V100% (100 W)
Experiment parameters:
|
Plasma Asher 4
Descum of AZ 5214E on 100 mm wafers. The descum process development was done for a single substrate, as well as 3 substrates (for decreased ashing rate and improved ashing uniformity). The substrates were placed vertically in the glass boat.
For the 3 substrates only the center substrate was used for testing, the front and back wafers were used as dummy wafers. The wafers were placed in consecutive slots - when running multiple wafers in this way, the first and last wafers should always be dummy wafers.
The user manual, risk assessment, and contact information can be found in LabManager - requires login
Typical descum parameters
Tested with 1.5 µm AZ 5214E on 100 mm silicon substrate.
- O2: 100 sccm
- N2: 100 sccm
- Pressure (DSC): 1.3 mbar
- Power: 200 W
- Chamber temperature at start: 30°C
- Time (single wafer): 5-10 minutes = 35-72 nm ashed
- Time (multiple wafers): 10-15 minutes = 40-80 nm ashed
| Test setup | Single substrate | Center of 3 substrates |
|---|---|---|
| Test results | Ashing rate: 5.7 ±2.1 nm/min Non-uniformity: 0.6 ±0.4% |
Ashing rate: 3.8 ±1.6 nm/min Non-uniformity: 0.4 ±0.2% |
| Wafers | 1 | 3 |
| Wafer size | 100 mm | 100 mm |
| Boat position | Center of chamber | Center of chamber |
| Test wafer position | Center of boat | Center of boat |
| Total gas flow rate | 200 sccm | 200 sccm |
| Gas mix ratio | 50% N2 | 50% N2 |
| Chamber pressure | 1.3 mbar | 1.3 mbar |
| Power | 200 W | 200 W |
| Test processing time | Tested parameter | Tested parameter |
| Test average temperature | 33°C | 33°C |
Single wafer ashing rate an uniformity

| Ashing time [min]: | 1 | 2 | 5 | 10 | 15 |
|---|---|---|---|---|---|
| Ashing amount [nm]: | 5.2 | 6.2 | 35.1 | 72.3 | 87.1 |
| Ashing rate [nm/min]: | 5.2 | 3.1 | 7.0 | 7.2 | 5.8 |
| Ashing time [min]: | 1 | 2 | 5 | 10 | 15 |
|---|---|---|---|---|---|
| Pre-descum film thickness range [nm]: | 11 | 12 | 10 | 11 | 9 |
| Pre-descum non-uniformity [%]: | 0.37 | 0.40 | 0.33 | 0.37 | 0.30 |
| Post-descum film thickness range [nm]: | 10 | 10 | 12 | 19 | 33 |
| Post-descum non-uniformity [%]: | 0.33 | 0.33 | 0.41 | 0.66 | 1.18 |
Multi wafer ashing rate and uniformity

| Ashing time [min]: | 1 | 2 | 5 | 10 | 15 |
|---|---|---|---|---|---|
| Ashing amount [nm]: | 4.3 | 6.7 | 10.1 | 39.5 | 78.8 |
| Ashing rate [nm/min]: | 4.3 | 3.4 | 2.0 | 4.0 | 5.3 |
| Ashing time [min]: | 1 | 2 | 5 | 10 | 15 |
|---|---|---|---|---|---|
| Film thickness range, before descum [nm]: | 11 | 13 | 11 | 12 | 14 |
| Pre-ashing non-uniformity [%]: | 0.37 | 0.43 | 0.37 | 0.40 | 0.46 |
| Film thickness range, after descum [nm]: | 11 | 9 | 10 | 12 | 21 |
| Post-ashing non-uniformity [%]: | 0.37 | 0.30 | 0.33 | 0.41 | 0.74 |
Comparison between single substrate processing and multi substrate processing
Processing a single substrate using the standard descum settings will provide users with a relatively controllable and uniform process. Adding dummy substrates in close proximity with the process substrate will reduce the ashing rate and improve the uniformity:
-
Ashing amount
-
Ashing rate
-
Non-uniformity
Plasma Asher 5
Plasma asher 5 is identical to plasma asher 4, see descum processing for plasma asher 4 here.