New page: == The nano1.43 recipe == {| border="2" cellpadding="2" cellspacing="1" |+ '''Recipe nano1.43''' |- ! rowspan="6" align="center"| Recipe | Gas | C<sub>4</sub>F<sub>8</sub> 75 sccm, SF<su... |
|||
| Line 44: | Line 44: | ||
C4F8 75 sccm, SF6 38 sccm, 4 mTorr, Strike 3 secs @ 15 mTorr, 800 W CP, 30 W PP, -20 degs, 120 secs | C4F8 75 sccm, SF6 38 sccm, 4 mTorr, Strike 3 secs @ 15 mTorr, 800 W CP, 30 W PP, -20 degs, 120 secs | ||
</gallery> | </gallery> | ||
{| {{table}} | |||
| align="center" style="background:#f0f0f0;"|'''Nominal trench line width''' | |||
| align="center" style="background:#f0f0f0;"|'''''' | |||
| align="center" style="background:#f0f0f0;"|'''30''' | |||
| align="center" style="background:#f0f0f0;"|'''60''' | |||
| align="center" style="background:#f0f0f0;"|'''90''' | |||
| align="center" style="background:#f0f0f0;"|'''120''' | |||
| align="center" style="background:#f0f0f0;"|'''150''' | |||
| align="center" style="background:#f0f0f0;"|'''Average''' | |||
| align="center" style="background:#f0f0f0;"|'''Std. dev.''' | |||
|- | |||
| Etch rates||nm/min||139||147||149||152||152||148||6 | |||
|- | |||
| Sidewall angle||degs||90||90||90||90||90||90||0 | |||
|- | |||
| CD loss||nm/edge||6||-21||-21||-41||-45||-24||21 | |||
|- | |||
| CD loss foot||nm/edge||11||-8||-8||-28||-18||-10||14 | |||
|- | |||
| Bowing||||1||-1||1||1||0||0||1 | |||
|- | |||
| Bottom curvature||||-50||-47||-34||-32||-31||-39||9 | |||
|- | |||
| zep||nm/min||||||||||||55|| | |||
|- | |||
| | |||
|} | |||