Jump to content

Specific Process Knowledge/Etch/ICP Metal Etcher/Chromium/End point: Difference between revisions

From LabAdviser
Bghe (talk | contribs)
Bghe (talk | contribs)
Line 55: Line 55:
|-
|-
|
|
<gallery caption="S047670 30 s barc etch, 7:45 min Cr etch, Feb-2025, wafer center, 100 nm Cr mask, with 500 nm resist" widths="600px" heights="550px" perrow="1">
<gallery caption="S047670 1 min barc etch, 7:45 min Cr etch, Feb-2025, wafer center, 100 nm Cr mask, with 500 nm resist" widths="600px" heights="550px" perrow="1">


File:S047670midt_cr_05.jpg
File:S047670midt_cr_05.jpg
Line 68: Line 68:


|
|
<gallery caption="S047670 30 s barc etch, 7:45 min Cr etch, Feb-2025, wafer edge, 100 nm Cr mask, with 500 nm resist" widths="600px" heights="550px" perrow="1">
<gallery caption="S047670 1 min barc etch, 7:45 min Cr etch, Feb-2025, wafer edge, 100 nm Cr mask, with 500 nm resist" widths="600px" heights="550px" perrow="1">


File:S047670edge_cr_01.jpg
File:S047670edge_cr_01.jpg

Revision as of 15:58, 18 February 2025

Feedback to this page': click here


THIS PAGE IS UNDER CONSTRUCTION

Made by Berit bghe @ DTU Nanolab

Using the standard Cr etch recipe I was etching through 100 nm Cr on a 150 mm wafer it an etch load of 50%

I recorded the end point signal and tried three different stopping times to figure out when to stop the etch. I want to find out how I can use the end point signal to get the best etch result; Etch though - also in the small patterns without too much over etch.

I was looking at trenches with sizes ranging from 200 nm to 2 µm in width. The masking materials was negative DUV resist: NUV 2300-0.5 of approximately 500 nm. Here process flow can be seen here: File:Process_flow_for_test_wafers xx.pdf

Etched close to optimal

Middel of the wafer Close to wafer edge

Etched too long

Middel of the wafer Close to wafer edge


Etched too short

Middel of the wafer Close to wafer edge