Specific Process Knowledge/Etch/DRIE-Pegasus/nanoetch/nano141: Difference between revisions
Appearance
New page: == The nano1.41 recipe == {| border="2" cellpadding="2" cellspacing="1" |+ '''Recipe nano1.41''' |- ! rowspan="6" align="center"| Recipe | Gas | C<sub>4</sub>F<sub>8</sub> 75 sccm, SF<su... |
|||
| Line 36: | Line 36: | ||
<gallery caption="The results of the nano1. | <gallery caption="The results of the nano1.41 recipe" widths="250" heights="200" perrow="3"> | ||
image:WF_2E07b_mar23_2011-030.jpg|The 30 nm trenches | image:WF_2E07b_mar23_2011-030.jpg|The 30 nm trenches | ||
image:WF_2E07b_mar23_2011-060.jpg|The 60 nm trenches | image:WF_2E07b_mar23_2011-060.jpg|The 60 nm trenches | ||
Revision as of 10:07, 2 May 2011
The nano1.41 recipe
| Recipe | Gas | C4F8 75 sccm, SF6 38 sccm |
|---|---|---|
| Pressure | 4 mTorr, Strike 3 secs @ 15 mTorr | |
| Power | 800 W CP, 75 W PP | |
| Temperature | -20 degs | |
| Hardware | 100 mm Spacers | |
| Time | 120 secs | |
| Conditions | Run ID | 2001 |
| Conditioning | Sequence: Oxygen clean, MU tests, processes, no oxygen between runs | |
| Mask | nm zep etched down to 6dgh4 nm |
- The results of the nano1.41 recipe
-
The 30 nm trenches
-
The 60 nm trenches
-
The 90 nm trenches
-
The 120 nm trenches
-
The 150 nm trenches