If 5214E is baked after exposure, the exposed resist will cross-link, making it insoluble in the developer. This is called the "Reversal bake". The reversal bake activates cross-linking of the exposed areas, which "reverses" the polarity of the design.
If 5214E is baked after exposure, the exposed resist will cross-link, making it insoluble in the developer. This is called the "Reversal bake". The reversal bake activates cross-linking of the exposed areas, which "reverses" the polarity of the design. When the substrate is flood-exposed after the reversal bake, the previously unexposed areas become soluble, and will be removed in the subsequent development. The image reversal procedure effectively makes AZ 5214E a negative resist.
 
If the substrate is flood exposed after the reversal bake, the previously unexposed areas become soluble, and will be removed in the subsequent development. The reversal procedure effectively makes AZ 5214E a negative resist.


The image reversal process greatly increases the sensitivity of AZ 5214E, and the dose of the image exposure is a critical parameter, especially if negative angled resist sidewalls are desired.<br>
The image reversal process greatly increases the sensitivity of AZ 5214E, and the dose of the image exposure is a critical parameter, especially if negative angled resist sidewalls are desired.<br>
Half dose of the normal, positive process is a good starting point for optimization. Similarly, the reversal bake is also a critical step, and must be tightly controlled in order to achieve consistent results. If negative sidewalls are desired, 60-120s at 110°C is recommended (as well as a resist thickness above 2 µm), but if straight sidewalls are desired, 60-120s at 120°C can be used.  
Half dose of the normal, positive process is a good starting point for optimization. Similarly, the reversal bake is also a critical step, and must be tightly controlled in order to achieve consistent results. If negative sidewalls are desired, 60 - 120 s at 110°C is recommended (as well as a resist thickness above 2 µm), but if straight sidewalls are desired, 60 - 120 s at 120°C can be used.  


The flood exposure, on the other hand, is uncritical, and 2-5 times the normal positive process dose is generally used.
The flood exposure, on the other hand, is uncritical, and ~5 times the normal positive process dose is generally used.


==Development==
==Development==
'''Development speed:'''
'''Development speed:'''
*Puddle development in 2.38% TMAH (AZ 726 MIF): ~2 µm/min
*Puddle development in 2.38% TMAH (AZ 726 MIF): ~2 µm/min

Revision as of 14:25, 5 April 2023

Specific Process Knowledge/Lithography/authors generic

Feedback to this page: click here

Resist description

AZ 5214E is a positive UV photoresist with image reversal capability. It is considered to have good adhesion when wet etching.

Spin coating

Spin curves for AZ 5214E using a 30 s spin-off, and a 60s @ 90°C softbake

Typical spin parameters:

  • Spin off: 30-60 s
  • Soft bake: 60 s @ 90°C


Image reversal

Typical image reversal parameters:

  • Reversal bake temperature: 110°C
  • Reversal bake time: 60 s
  • Flood exposure: 500 mJ/cm2


If 5214E is baked after exposure, the exposed resist will cross-link, making it insoluble in the developer. This is called the "Reversal bake". The reversal bake activates cross-linking of the exposed areas, which "reverses" the polarity of the design. When the substrate is flood-exposed after the reversal bake, the previously unexposed areas become soluble, and will be removed in the subsequent development. The image reversal procedure effectively makes AZ 5214E a negative resist.

The image reversal process greatly increases the sensitivity of AZ 5214E, and the dose of the image exposure is a critical parameter, especially if negative angled resist sidewalls are desired.
Half dose of the normal, positive process is a good starting point for optimization. Similarly, the reversal bake is also a critical step, and must be tightly controlled in order to achieve consistent results. If negative sidewalls are desired, 60 - 120 s at 110°C is recommended (as well as a resist thickness above 2 µm), but if straight sidewalls are desired, 60 - 120 s at 120°C can be used.

The flood exposure, on the other hand, is uncritical, and ~5 times the normal positive process dose is generally used.

Development

Development speed:

  • Puddle development in 2.38% TMAH (AZ 726 MIF): ~2 µm/min