=Recipes on PECVD2 for deposition of silicon oxides=
===Recipes===
{| border="1" cellspacing="0" cellpadding="7"
|-
|Recipe name
|SiH4 flow [sccm]
|N<math>_2</math>O flow [sccm]
|N2 flow [sccm]
|Pressure [mTorr]
|Power [W]
|Description
|-
|1STOxide
|12
|1420 (setting in software is 710)
|392
|550
|100
|
|-
|}
LF=Low Frequency
===Expected results===
{| border="1" cellspacing="0" cellpadding="5"
|-
|Recipe name
|Deposition rate [nm/min]
|RI
|Uniformity [%]
|-
|STOxide
|[[/deposition rate for STOxide|~100]]
|~1.47
|<1
|-
|}


=Recipes on PECVD3 for deposition of silicon oxides=
=Recipes on PECVD3 for deposition of silicon oxides=

Revision as of 17:43, 8 November 2010

At the moment DANCHIP has 3 PECVDs that can deposite silicon oxide with or without dopants of Boron, Phosphorous or Germanium. PECVD1 and PECVD3 are for silicon based processing. PECVD2 is for III-V processing and will be describes under III-V processing. Look at the PECVD page to learn more about the PECVDs at DANCHIP. All though PECVD1 and PECVD3 are very much alike you cannot count on the a recipe on one system will give exactly the same results on the other system.


Recipes on PECVD1 for deposition of silicon oxides

Recipes

Recipe name SiH4 flow [sccm] N2O flow [sccm] N2 flow [sccm] B2H6 flow [sccm] PH3 flow [sccm] Pressure [mTorr] Power [W] Description
1oxide/standard 17 1600 0 0 0 400 380LF Developed for waveguides
1PBSG Developed for waveguide top cladding by Haiyan Ou @DTU Photonics

Expected results

Recipe name Deposition rate [µm/min] RI Uniformity [%]
1oxide/standard ~0.193 1.46 2
1PBSG ~0.3


Recipes on PECVD3 for deposition of silicon oxides

Recipes

Recipe name SiH4 flow [sccm] N2O flow [sccm] N2 flow [sccm] Pressure [mTorr] Power [W] Description
LFSiO 12 1420 392 550 60

LF=Low Frequency

Expected results

Recipe name Deposition rate [nm/min] RI Uniformity [%]
LFSiO ~81 ~1.48 <1