Jump to content

Specific Process Knowledge/Characterization/AFM: Atomic Force Microscopy/AFM Icon Acceptance: Difference between revisions

From LabAdviser
Bghe (talk | contribs)
Bghe (talk | contribs)
Line 225: Line 225:
*#*Peak force frequency: 2 Hz
*#*Peak force frequency: 2 Hz
*#*Rq: 0.247 nm
*#*Rq: 0.247 nm
[[File:Roughness on Si 1 ScanAsyst with ScanAsyst-air CL on.JPG|400px]]
*#ScanAsyst with ScanAsyst-air
*#ScanAsyst with ScanAsyst-air
*#*CL off
*#*CL off
Line 233: Line 234:
*#*Peak force frequency: 2 Hz
*#*Peak force frequency: 2 Hz
*#*Rq: 0.235 nm
*#*Rq: 0.235 nm
[[File:Roughness on Si 2 ScanAsyst with ScanAsyst-air CL off.JPG|400px]]
*#ScanAsyst with TAP150A
*#ScanAsyst with TAP150A
*#*CL on
*#*CL on
Line 238: Line 240:
*#*0dg
*#*0dg
*#*ScanAsyst noise threshold: 1
*#*ScanAsyst noise threshold: 1
*#*PeakForce amplitide 75 nm (was set as standard from the probe settings)
*#*PeakForce amplitude 75 nm (was set as standard from the probe settings)
*#*Peak force frequency: 2 Hz
*#*Peak force frequency: 2 Hz
*#*Rq: 0.238/0.250 nm
*#*Rq: 0.238/0.250 nm
[[File:Roughness on Si 3 ScanAsyst with TAP150A CL on A.JPG|400px]][[File:Roughness on Si 3 ScanAsyst with TAP150A CL on B.JPG|400px]]
*#Tapping mode with TAP150A
*#Tapping mode with TAP150A
*#*CL on
*#*CL on
Line 246: Line 249:
*#*0dg
*#*0dg
*#*Rq: 0.214 nm
*#*Rq: 0.214 nm
[[File:Roughness on Si 4 Tapping mode with TAP150A CL on.JPG|400px]]
*#Tapping mode with RFESP-75
*#Tapping mode with RFESP-75
*#*CL on
*#*CL on
Line 251: Line 255:
*#*0dg
*#*0dg
*#*Rq: 0.224 nm
*#*Rq: 0.224 nm
[[File:Roughness on Si  5 Tapping mode with RFESP-75 CL on.JPG|400px]]

Revision as of 16:55, 18 May 2020

Feedback to this page: click here

Accessories following the systems

Equipment AFM Icon AFM Icon 2
Chucks
  • A symmetric chuck that handles up to 210mm wafers and 15mm thick
  • An asymmetric chuck that handles up to ~4" wafer (but not small pieces) - using this a whole 4" can be accessed without rotating the sample.
  • A symmetric chuck that handles up to 210mm wafers and 15mm thick
Holders
  • Magnetic sample holder + magnetic discs + double sided tape
  • Holder for vertical profile scans
  • Magnetic sample holder + magnetic discs + double sided tape
  • Holder for vertical profile scans ?
Modes included
  • PeakForce Tapping mode / ScanAsyst
  • TappingMode (air)
  • Contact Mode
  • Lateral Force Microscopy
  • Phase Imaging
  • Lift mode
  • MFM
  • Force Spectroscopy
  • Force volume
  • EFM
  • surface potential
  • Torsional Resonance Mode
  • Piezoresponse Microscopy
  • Force spectroscopy


Extra modes:

  • PeakForce KPFM package (incl extra box for high voltage PF KPFM)
  • PFQNM package
  • Microscope Image Registration and Overlay (MIRO) software. this is only working in the old software (before version 9.4)
  • PeakForce Tapping mode / ScanAsyst
  • TappingMode (air)
  • Contact Mode
  • Lateral Force Microscopy
  • Phase Imaging
  • Lift mode
  • Force Spectroscopy
  • Force volume
  • surface potential
  • Torsional Resonance Mode
  • Piezoresponse Microscopy
  • Force spectroscopy


Probes that followed the systems
ScanAsyst mode Tapping mode Contact mode PF-KPFM
  • ScanAsyst air 30ps
  • ScanAsyst fluid 10ps
  • ScanAsyst fluid + 10ps
  • MPP-11100-10
  • MPP-21100-10
  • MPP-11120-10 RTESPA
  • TESPA-V2 10ps
  • OTESPA-R3 10ps
  • High Aspect ratio probes 1:15: FIB6-400A 5ps
  • MPP-12120 10ps. Tap150A
  • MPP-13120-10 TAP525A
  • SNL-10 20ps
  • SCM-PIT 10ps
  • PFQNE-Al 10ps
ScanAsyst mode Tapping mode Contact mode
  • ScanAsyst air 20ps
  • ScanAsyst fluid 10ps
  • ScanAsyst fluid + 10ps
  • RTESP-300 (like MPP-11100-10)
  • RFESP-75 (like MPP-21100-10)
  • TESPA-V2 10ps
  • OTESPA-R3 10ps
  • NCHV 10ps
  • SNL-10 20ps
Samples
  • QC grid: VGRP-15M 10µm pitch and depth reference 178nm
  • PF KPFM-SMPL Kelvin probe Sample: Al + Au on Si
  • HOPG: Highly Oriented Pyrolytic Graphite

Calibration samples for getting quantitative modulus measurements:

  1. PDMS-soft-1-12M: PDMS gel 2.5MPa
  2. PDMS-soft-2-12M: PDMS gel 3.5MPa
  3. PSFilm-12M: Polystyrene filem
  4. FSilica-12M: Fused Silica
  5. Sapphire-12M: Sapphire
  6. RS-12M: Ti roughness sample
  7. HOPG-12M: Highly Orientated Pyrolytic Graphite
  8. PS-LDPE: Harmonix training
  • QC grid: VGRP-15M 10µm pitch and depth reference 181nm
  • HOPG: Highly Oriented Pyrolytic Graphite


AFM Icon-Pt 1: Acceptance tests done

Noise tests

Sensor noise

Tappingmode, OTESPA-R3 probe used.
First we made a false engage (scanning in air): Turn off gain 0 0
Z range 0.2my
Scan size 0.01nm
We saw some 50Hz noise (electrical - or maybe pumps): Rq 15 pm (specs 35pm)


System noise

Noise on sample: scan size 0.1nm
we started with 1my scan size to optimize the scan.
2.43Hz
256 lines
Z range at 2my to get sub nanometer resolution in Z
Rq: 54,5pm (plade vibrator koerte udenfor)
Rq: 23pm uden vibrator koerende + ro og med aaben hood.
Rq:71pm uden vibrator koerende + ro og med lukket hood


Roughness

HAR: 200nm wide 400nm deep

HAR: 2µm wide 6µm deep

Graphene KPFM measurement


Height image: The graphene and structuring in graphene is not visible
Potential image: Potential difference between grapheme and non-graphene is visible
Phase: Phase imaging maps the phase lag between the periodic signal driving the cantilever and the oscillations of the cantilever. Changes in phase lag often indicate changes in the properties of the sample surface. Here the structuring in the graphene is very clear

AFM Icon-Pt 2: Acceptance test

Noise tests

Sensor noise

Tapping ]mode, OTESPA-R3 probe used.
First we made a false engage (scanning in air): Turn off gain 0 0
Z range 0.2my
Scan size 0.01nm
Roughness: Rq 28 pm (specs 35pm)


System noise

Noise on sample: scan size 0.1nm
we started with 1my scan size to optimize the scan.
2.43Hz
256 lines
Z range at 2my to get sub nanometer resolution in Z
Rq: 28 pm


Demonstrating roughness measurements on silicon

    1. ScanAsyst with ScanAsyst-air
      • CL on
      • 512x512
      • 0dg
      • ScanAsyst noise threshold: 1
      • PeakForce amplitide 300 nm
      • Peak force frequency: 2 Hz
      • Rq: 0.247 nm

    1. ScanAsyst with ScanAsyst-air
      • CL off
      • 512x512
      • 0dg
      • ScanAsyst noise threshold: 0.2
      • PeakForce amplitide 300 nm
      • Peak force frequency: 2 Hz
      • Rq: 0.235 nm

    1. ScanAsyst with TAP150A
      • CL on
      • 512x512
      • 0dg
      • ScanAsyst noise threshold: 1
      • PeakForce amplitude 75 nm (was set as standard from the probe settings)
      • Peak force frequency: 2 Hz
      • Rq: 0.238/0.250 nm

    1. Tapping mode with TAP150A
      • CL on
      • 512x512
      • 0dg
      • Rq: 0.214 nm

    1. Tapping mode with RFESP-75
      • CL on
      • 512x512
      • 0dg
      • Rq: 0.224 nm