== Standard process parameter monitoring ==
== Standard process parameter monitoring ==


The original standard recipes on Pegasus 1 differ in many ways. The second step of one of them is listed below:
The original standard recipes on Pegasus 1 differ in many ways. Here, we go through two of them.
 
=== Process A ===
 
The process parameters of the second step of Process A is listed in the table below:


{| {{table}}
{| {{table}}
Line 43: Line 47:
|-
|-
|}
|}
When running any recipe on the SPTS Pro software, a set of process parameters are recorded as the process runs. This data can be accessed later by looking up the datalog. Which parameters are recorded is dictated by the socalled logging recipe that is selected for every process recipe. The list of possible parameters to include in a logging recipe is long and is comprised of both input parameters such as 'Coil forward power demand' and 'SF<sub>6</sub> flow setpoint', and measured values such as 'Platen temperature' and 'Platen DC Bias'. During the process itself, one can also activate the 'Trace' to monitor the process parameters in real time.  
When running any recipe on the SPTS Pro software, a set of process parameters are recorded as the process runs. This data can be accessed later by looking up the datalog. Which parameters are recorded is dictated by the so-called logging recipe that is selected for every process recipe. The list of possible parameters to include in a logging recipe is long and is comprised of both input parameters such as 'Coil forward power demand' and 'SF<sub>6</sub> flow setpoint', and measured values such as 'Platen temperature' and 'Platen DC Bias'. During the process itself, one can also activate the 'Trace' to monitor the process parameters in real time.  


To the left in the figure below, some of the most important process parameters are shown for a process run of the recipe Process A.
To the left in the figure below, some of the most important process parameters are shown for a process run of the recipe Process A.
Line 66: Line 70:
** The reading of the DC Bias has much more detail than the one-point reading of the Pro software indicates.
** The reading of the DC Bias has much more detail than the one-point reading of the Pro software indicates.
* There are oscillations in the pressure every time whenever there is a change of gas flow
* There are oscillations in the pressure every time whenever there is a change of gas flow
Since Process A is a standard recipe we will not change it as it is. Before deciding what to do we'll have a look at another recipe with shorter cycles.
=== Process D4 ===
{| {{table}}
{| border="1" cellspacing="0" cellpadding="1"  align="center"
! colspan="3" |[[Specific Process Knowledge/Etch/DRIE-Pegasus/processD#The_new_standard_process_Process_D4 |Process D4 ]]
|-
! Parameter 
! Etch
! Dep
|-
! Gas flow (sccm)
| SF<sub>6</sub> 275, O<sub>2</sub>
| C<sub>4</sub>F<sub>8</sub> 150
|-
! Cycle time (secs)
| 2.2
| 1
|-
! Pressure (mtorr)
| 26
| 20
|-
! Coil power (W)
| 2500
| 2000
|-
! Platen power (W)
| 35
| 0
|-
! Common
| colspan="2" | Temperature 0 degs
|-
|}





Revision as of 12:29, 18 March 2020

Feedback to this page: click here

Process optimization using the Picoscope

Before going into details on why it makes sense to optimize the processes using the picoscope process monitoring, we need to have a look at how monitoring processes is usually done.

Standard process parameter monitoring

The original standard recipes on Pegasus 1 differ in many ways. Here, we go through two of them.

Process A

The process parameters of the second step of Process A is listed in the table below:

Process A Step 2 parameters
Parameter Etch Dep
Gas flow (sccm) SF6 350 (1.5 s), 550 C4F8 200
Cycle time (secs) 7.0 4.0
Pressure (mtorr) 25 (1.5 s), 150 25
Coil power (W) 2800 2000
Platen power (W) 140 (1.5) 45 0
Common Temperature 20 degs

When running any recipe on the SPTS Pro software, a set of process parameters are recorded as the process runs. This data can be accessed later by looking up the datalog. Which parameters are recorded is dictated by the so-called logging recipe that is selected for every process recipe. The list of possible parameters to include in a logging recipe is long and is comprised of both input parameters such as 'Coil forward power demand' and 'SF6 flow setpoint', and measured values such as 'Platen temperature' and 'Platen DC Bias'. During the process itself, one can also activate the 'Trace' to monitor the process parameters in real time.

To the left in the figure below, some of the most important process parameters are shown for a process run of the recipe Process A.

Above to the left, one can see the multiplexing of the Bosch process by alternation of the gas flows of SF6 (that has flow initially at 350 sccm in the break for the first 1.5 second then 550 sccm for 5.5 seconds in the main etch phase) and C4F8 (at 200 sccm in the dep phase) according to the process recipe table above. Below, the Pressure alternates between 25 mtorr (dep and break) and 150 mtorr (main). The Platen Electrode DC Bias (the electrostatic potential difference between the plasma and the wafer electrode that drives the ion bombardment in the etch process) is generated by the Platen Power at 140 W in the break and 45 W in the main etch. Below this, the Reflected Platen Power is not zero. The Coil Power is 2800 W (etch) and 2000W (dep) with the Reflected Coil Power below. The spikes in Coil Power at every point where the Reflected is not zero indicates that the Coil Power is running in Load mode (as opposed to Forward mode) where the power lost as reflected power is compensated for by increasing the input power.

Process A has 4 second dep phase and 7 second (1.5 second break and 5.5 second main) and the SPTS Pro software samples the process parameters every 0.5 second. This produces plots as seen above where all measurements have markers. One can ask the questions:

  1. What happens if the cycle duration is lowered in order produce smaller scallops?
  2. How do we know if something that is very brief happens? For instance, spikes in reflected power can be rather short lived as indicated by the one point spikes of reflected coil power above.

In both cases, the sampling frequency of 2 Hz is simply not high enough - we need to increase this. The SPTS Pro software can only lower this. However, realizing that all the devices (mass flow controllers, pressure gauges, RF generators etc.) responsible for the parameters in the plot above are produce output measurements in real time, we can sample these parameters by some external device. Enter the Picoscope oscilloscope with 8 analog channels that enable us sample up to 8 outputs, usually a DC voltage, at almost any sampling rate. Unlike the old oscilloscopes, the Picoscope is fully operated by a software that produces a vast amount of data and nice plots. We therefore have to decide which process parameters are the most important to monitor and then go through the electrical diagrams to find an appropriate place to pick up the signal. This set of parameters is chosen as shown in the plots above.

Comparing the two plots we observe the following:

  • There is, indeed, short lived incidences that are not picked up by the SPTS Pro software:
    • Spikes of high flow when the C4F8 MFC opens.
    • Spikes of reflected coil power.
    • The reading of the DC Bias has much more detail than the one-point reading of the Pro software indicates.
  • There are oscillations in the pressure every time whenever there is a change of gas flow

Since Process A is a standard recipe we will not change it as it is. Before deciding what to do we'll have a look at another recipe with shorter cycles.

Process D4

Process D4
Parameter Etch Dep
Gas flow (sccm) SF6 275, O2 C4F8 150
Cycle time (secs) 2.2 1
Pressure (mtorr) 26 20
Coil power (W) 2500 2000
Platen power (W) 35 0
Common Temperature 0 degs


zx