The Anneal-bond furnace (C3) is a Tempress horizontal furnace for oxidation and annealing of new and processed (e.g. bonded) silicon wafers. O2 is used as an oxidant for dry oxidation, and for wet oxidation water vapour is being generated by a bubbler.  
The Anneal-bond furnace (C3) is a Tempress horizontal furnace for oxidation and annealing of new and processed (e.g. bonded) silicon wafers. O<sub>2</sub>) is used as an oxidant for dry oxidation, and for wet oxidation water vapour is being generated by a bubbler.  


This furnace is the third tube in the furnace C-stack positioned in cleanroom B-1.  
This furnace is the third tube in the furnace C-stack positioned in cleanroom B-1.  

Revision as of 15:38, 30 January 2020

Feedback to this page: click here

Anneal-bond furnace (C3)

Anneal-bond furnace (C3). Positioned in cleanroom B-1

The Anneal-bond furnace (C3) is a Tempress horizontal furnace for oxidation and annealing of new and processed (e.g. bonded) silicon wafers. O2) is used as an oxidant for dry oxidation, and for wet oxidation water vapour is being generated by a bubbler.

This furnace is the third tube in the furnace C-stack positioned in cleanroom B-1.

In this furnace it is allowed oxidize and anneal new wafers without doing an RCA clean first. Also silicon wafers from PECVD4 and wafers without any metal coming from PECVD3 and bonded wafers comming directly from the Wafer Bonder 02 (assuming they were clean and not have been exposed to any metal when entering wafer bonder) can be processed in the furnace without an RCA cleaning. Check the cross contamination information in LabManager before you use the furnace.


The user manual, technical information and contact information can be found in LabManager:

Anneal-bond Furnace (C3)

Process knowledge

Overview of the performance of Anneal Bond furnace and some process related parameters

Purpose
  • Oxidation of Si wafers
  • Annealing of processed wafers, eg. bonded wafers from EVG NIL
Oxidation:
  • Dry
  • Wet: with bubbler (water steam + O2)
Performance Film thickness
  • Dry SiO2: 50 Å to ~2000 Å (it takes too long to grow a thicker oxide)
  • Wet SiO2: 50 Å to ~5 µm (it takes too long to grow a thicker oxide)
Process parameter range Process temperature
  • 800-1150 oC
Process pressure
  • 1 atm
Gas flows
  • N2: 0-10 slm
  • O2: 0-10 slm
Substrates Batch size
  • 1-30 100 mm wafers (or 50 mm wafers) per run
Substrate materials allowed
  • Silicon wafers (new wafers or RCA cleaned wafers)
  • Silicon wafers with layers of silicon oxide or silicon (oxy)nitride (RCA cleaned)
  • Wafers from the LPCVD furnaces
  • Wafers from PECVD4
  • Wafers from PECVD3 (without any metal)
  • Wafers from Wafer Bonder 02 (assuming they were clean and not have been exposed to any metal when entering the Wafer Bonder 02)