he FEI Nova 600 NanoSEM Scanning Electron Microscope is a very versatile characterization instrument that produces enlarged images of a variety of specimens, achieving magnifications of over 500.000 times providing ultra high resolution imaging. At the time being this microscope is mainly designated for microstructural characterization using electron backscatter diffraction (EBSD) , Energy-dispersive X-ray spectroscopy (EDS) and forward scatter electron imaging by detect
= Kikuchi lines =
 
The formation of Kikuchi patterns can be described as a two-step process, as shown schematically in Fig. 3.1. The fi�rst step consists of an incoherent inelastic, large angle scattering process of the primary beam electrons, producing a point-like electron source inside of the crystal. The second step is the elastic and inelastic coherent
scattering of these electrons by the crystal planes of the material: the electrons can be Bragg reflected at lattice planes with reciprocal lattice vector -g if the Bragg angle is ±B or if the direction of incidence ~ k_0 lies on one of the Kossel cones, which have an aperture 90°- �~B and the ~g direction (normal to the lattice planes) as axis. There is a pair of Kossel cones for ~g, another pair for 2~g and so on. The intersection between the Kossel cones and the plane of observation results in the formation of Kikuchi lines. The intersection is an hyperbola, but the lines are approximately straight owing to the low value of �~B . The formed Kikuchi lines do not have the same intensity: one line, called the excess line, is brighter than the other, called the defect line.
 
An example of a formed Kikuchi pattern is visible in Fig. 3.3, showing the excess (bright) and defect (black) Kikuchi lines and a zone axis, indicating an intersection of planes.
 
= Indexing of Kikuchi patterns =
 
The automated determination of the position of Kikuchi lines in a di�raction
pattern (and consequently of lattice planes in the crystal) has enabled
the practical use of Kikuchi di�raction for the study of micro- and nanomaterials.
An algorithm known as the Hough transform was introduced by
The simple geometry of Kikuchi di�raction makes indexing and orientation
determination from Kikuchi patterns straightforward: the position of
the di�racting lattice plane in the crystal can be easily determined from the
center line of a pair of Kikuchi lines, together with the lattice plane spacing
from the distance between the lines themselves.
 
Krieger Lassen to recognize the edges of the Kikuchi bands [27, 28]. The
Hough transform is a mathematical tool which can be used to isolate features
of a particular shape, such as lines, circles and ellipses, within an
image. The main advantage of the Hough transform is that it is relatively
una�ected by image noise. The essential idea of the the Hough transform
consists of applying to each pixel of the Kikuchi pattern the equation:
�i = xcos�i + ysin�i (3.1)
where (x, y) are the coordinates of a pixel in the original image and (�i, �i)
are the parameters of a straight line passing through (x, y). From Eq. 3.1
it is evident that the set of possible lines passing through the chosen pixel
is represented by a sinusoid in the Hough space.
An example is shown in Fig. 3.4. Consider four pixels along a Kikuchi
line. For each pixel in the line, all possible values of � are calculated for �
ranging from 0° to 180° using Eq. 3.1, which produces four sinusoidal curves.
These curves intersect at a point with (�, �) coordinates (green rectangle),
corresponding to the angle of the line (�) and its position relative to the origin
(�). The grey-scale intensity I(xi; yi) of the image pixels is accumulated
in each quantized point H(�; �) of the Hough space, so that I(xi; yi) serves as
a measure of evidence for a line passing through the pixel (x, y). In this way,
a line in the pattern space transforms to a point having a certain intensity
in the Hough space, which is easily detected by the indexing software over
the
at background. For a correct indexing, the crystal system, chemical
composition, unit cell dimensions and atomic positions of the material must
be supplied to the analysis software.
 
In a Kikuchi pattern, a set of orientations is obtained from a triplet of
bands by measuring the interplanar angles between the bands. These values
are compared against theoretical values of all angles formed by various planes
for a given crystal system. When the (h, k, l ) values of a pair of lines are
identi�ed, they give information about the pair of planes, but that does
 
not permit to distinguish between the two planes. At least three sets of
lines are required to completely identify the individual planes and hence to
�nd the orientation of the sample. For a given number of bands, n, used for
pattern indexing, the number of band triplets is determined by the following
formula:
N:triplets =
n!
(n 􀀀 3)! � 3!
(3.2)
Typically from 3 to 9 detected bands are used for automatic indexing in
commercial softwares.