====Experimental setup==== | ====Experimental setup==== | ||
''' | ''' | ||
20 boron doped device wafers (p-type) were used - Four wafers for each of the five different predeposition temperatures (see table below). In the furnace five dummy wafers were placed on each side of the device wafers. The dummy wafers nearest to the device wafers were changed in-between the runs to | 20 boron doped device wafers (p-type) were used - Four wafers for each of the five different predeposition temperatures (see table below). In the furnace five dummy wafers were placed on each side of the device wafers. The dummy wafers nearest to the device wafers were changed in-between the runs to minimize doping from these dummy wafers. | ||
{| border="1" cellspacing="1" cellpadding="2" style="text-align:center;" width="690" ||3||4||5 | {| border="1" cellspacing="1" cellpadding="2" style="text-align:center;" width="690" ||3||4||5 | ||
!| Run #||Temperature||Process time with POCl<sub>3</sub>||Annealing time in O<sub>2</sub>||Wafer # | !| Run #||Temperature||Process time with POCl<sub>3</sub>||Annealing time in O<sub>2</sub>||Wafer # | ||
|- | |- | ||
|1||850 <sup>o</sup>C||15 minutes||20 | |1||850 <sup>o</sup>C||15 minutes||20 minutes||1, 2, 3, 4 | ||
|- | |- | ||
|2||900 <sup>o</sup>C||15 minutes||20 | |2||900 <sup>o</sup>C||15 minutes||20 minutes||5, 6, 7, 8 | ||
|- | |- | ||
|3||950 <sup>o</sup>C||15 minutes||20 | |3||950 <sup>o</sup>C||15 minutes||20 minutes||9, 10, 11, 12 | ||
|- | |- | ||
|4||1000 <sup>o</sup>C||15 minutes||20 | |4||1000 <sup>o</sup>C||15 minutes||20 minuntes||13, 14, 15, 16 | ||
|- | |- | ||
|5||1050 <sup>o</sup>C||15 minutes||20 | |5||1050 <sup>o</sup>C||15 minutes||20 minutes||17, 18, 19, 20 | ||
|} | |} | ||
''' | ''' | ||
| Line 53: | Line 53: | ||
! width="130" | Temperature [C] | ! width="130" | Temperature [C] | ||
! width="130" | Oxide thickness [nm] | ! width="130" | Oxide thickness [nm] | ||
! width="130" | | ! width="130" | Refractive index | ||
! width="150" | Sheet resistance [Ω<sub>sq</sub>] | ! width="150" | Sheet resistance [Ω<sub>sq</sub>] | ||
! width="150" | Slice Resistivity [Ωcm] | ! width="150" | Slice Resistivity [Ωcm] | ||
| Line 107: | Line 107: | ||
! width="130" | Temperature [<sup>o</sup>C] | ! width="130" | Temperature [<sup>o</sup>C] | ||
! width="130" | Oxide thickness [nm] | ! width="130" | Oxide thickness [nm] | ||
! width="130" | | ! width="130" | Refractive index | ||
! width="150" | Sheet resistance [Ω<sub>sq</sub>] | ! width="150" | Sheet resistance [Ω<sub>sq</sub>] | ||
! width="150" | Slice Resistivity [Ωcm] | ! width="150" | Slice Resistivity [Ωcm] | ||
| Line 169: | Line 169: | ||
|} | |} | ||
Looking at the "SIMS Measurement After Drive-in Process at 1050 <sup>o</sup>C" graph, it can be seen that the two curves "Pre-dep at 950 <sup>o</sup>C" and "Pre-dep at 1000 <sup>o</sup>C" are crossing each other, but according to the theory they should not do that. Only one wafer has been | Looking at the "SIMS Measurement After Drive-in Process at 1050 <sup>o</sup>C" graph, it can be seen that the two curves "Pre-dep at 950 <sup>o</sup>C" and "Pre-dep at 1000 <sup>o</sup>C" are crossing each other, but according to the theory they should not do that. Only one wafer has been measured so there is not that much statistical data to verify it with. | ||
==Test of the Phosphorus Predep furnace== | ==Test of the Phosphorus Predep furnace== | ||
| Line 176: | Line 176: | ||
''' | ''' | ||
To find the result of a specific process using the Phosphorus Predep furnace (A4) followed by a drive in and oxidating the substrate in the | To find the result of a specific process using the Phosphorus Predep furnace (A4) followed by a drive in and oxidating the substrate in the Phosphorus drive in furnace (A3). | ||
''' | ''' | ||
Revision as of 16:41, 25 November 2019
Feedback to this page: click here
The Phosphorus Predep furnace (A4) can be used for phosphorus predeposition of silicon wafers, resulting in N-type doping. In the furnace, the silicon wafers are positioned vertically in a quarts boat.
Test of the Phosphorus Predep furnace
Purpose
To study the correlation between the temperature for the predeposition process and drive-in of the phosphorus doping in the Phosphorus Predep furnace (A4) at DTU Danchip.
Experimental setup
20 boron doped device wafers (p-type) were used - Four wafers for each of the five different predeposition temperatures (see table below). In the furnace five dummy wafers were placed on each side of the device wafers. The dummy wafers nearest to the device wafers were changed in-between the runs to minimize doping from these dummy wafers.
| Run # | Temperature | Process time with POCl3 | Annealing time in O2 | Wafer # |
|---|---|---|---|---|
| 1 | 850 oC | 15 minutes | 20 minutes | 1, 2, 3, 4 |
| 2 | 900 oC | 15 minutes | 20 minutes | 5, 6, 7, 8 |
| 3 | 950 oC | 15 minutes | 20 minutes | 9, 10, 11, 12 |
| 4 | 1000 oC | 15 minutes | 20 minuntes | 13, 14, 15, 16 |
| 5 | 1050 oC | 15 minutes | 20 minutes | 17, 18, 19, 20 |
After the predeposition two wafers from each run were taken out to be further processed. These wafers were: 1, 2, 5, 6, 9, 10, 13, 14, 17, 18. These wafers were dipped in BHF to remove the phosphorus glass layer before the drive-in process.
The drive-in process was made in the Phosphorus Drive-in furnace (A3) for all the mentioned wafers at same time. At the drive-in process a dummy wafer was placed in-between the wafers that have been predeposited at different temperatures, so doping from wafer to wafer was minimized. The phosphorus drive-in was done with the process "DRY1050" which is a dry oxidation at 1050 oC for 100 minutes and 20 minutes annealing. At the oxidation the O2 flow was 5 SLM, and the N2 flow for annealing was 3 SLM.
Results
Several measurements were done for the different device wafers. After the predeposition, the thickness of the grown phosphorus glass layer was measured, and the sheet resistance and slice resistivity were measured on the same wafer after a BHF etch.
| Ellipsometer (center point only) | Four Point Probe | ||||
|---|---|---|---|---|---|
| Wafer # | Temperature [C] | Oxide thickness [nm] | Refractive index | Sheet resistance [Ωsq] | Slice Resistivity [Ωcm] |
| 3 | 850 | 27,4 | 1,4623 | 311 | 6,22*10-3 |
| 7 | 900 | 45,27 | 1,4622 | 138,5 | 4,85*10-3 |
| 11 | 950 | 61,36 | 1,4625 | 16,1 | 1,29*10-3 |
| 15 | 1000 | 80,45 | 1,4624 | 7,4 | 0,89*10-3 |
| 19 | 1050 | 119,37 | 1,4623 | 6,6 | 1,49*10-3 |
The oxide layer was etch in BHF before the drive-in of the doping with a dry oxidation at 1050 oC for 100 minutes and 20 minutes annealing.
| Avg. five point on Filmtek | Four Point Probe | ||||
|---|---|---|---|---|---|
| Wafer # | Temperature [oC] | Oxide thickness [nm] | Refractive index | Sheet resistance [Ωsq] | Slice Resistivity [Ωcm] |
| 2 | 850 | 110,44 | 1,4654 | 189,7 | 3,79*10-3 |
| 6 | 900 | 116,28 | 1,4629 | 101,6 | 3,56*10-3 |
| 9 | 950 | 137,06 | 1,4604 | 10,0 | 0,8*10-3 |
| 14 | 1000 | 141,46 | 1,4651 | 4,72 | 0,57*10-3 |
| 18 | 1050 | 139,87 | 1,4659 | 3,23 | 0,73*10-3 |
| Blank Si wafer | 110,71 | 1,46286 | - | - | |
Looking at the "SIMS Measurement After Drive-in Process at 1050 oC" graph, it can be seen that the two curves "Pre-dep at 950 oC" and "Pre-dep at 1000 oC" are crossing each other, but according to the theory they should not do that. Only one wafer has been measured so there is not that much statistical data to verify it with.
Test of the Phosphorus Predep furnace
Purpose
To find the result of a specific process using the Phosphorus Predep furnace (A4) followed by a drive in and oxidating the substrate in the Phosphorus drive in furnace (A3).
Experimental setup
Substrate: p-type Si(100,)
Resistivity: 1-20 Ωcm
Recipe: POCL900
Temperature: 900 °C
Time: 15 min
Anneal: 20 min in N2
After removing the oxide in BHF the wafers were oxidized in Phosphor Drive in Furnace (A3) using DRY1050 at 1050°C for 70 min without further annealing in N2. Results are listed in the table below:
Results
| Afer predeposition | After Oxidation | ||
|---|---|---|---|
| Test date | Sheet resistance [Ω/sq] | Oxide thickness [nm] | Sheet resistance [Ω/sq |
| Aug2012 | 47.0 | 93.1 | 41.8 |
| Jan2013 | 50.5 | 91.3 | 55.6 |
| Aug2013 | 58.0 | 91.8 | 41.8 |
| Jan2014 | 54.1 | 93.3 | 33.8 |
| Jan2015 | 50.8 | 94.2 | 39.4 |
One wafer from Jan2015 was analyzed with SIMS and the profile is shown on the graph below:

Result from GreenBelt, @Danchip,Jan 2015
Test of the Phosphorus Predep furnace
Purpose
To find the doping profile after a specific process flow. The test was made by only performing the high-temperature process step after the pre-deposition step done in the Phosphorus Predep furnace (A4). The subsequently high temperature processes was done by using the Phosphorous drive in furnace (A3) and the Oxide Anneal Furnace (C3).
Experimental setup
Substrate: p-type Si(100,)
Resistivity: 1-20 Ωcm
The total thermal budget for the wafers:
Predeposition in Furnace (A4): POCL1000, 15 min, no further anneal
Wet Oxidation in Furnace (A3): WET1050, 30 min, no further anneal
Anneal in Furnace (C1): ANN1000, 30 min in N2
Wet oxidation in Furnace (C1): WET1050, 30 min, no further anneal
Results
The wafer was analyzed with SIMS and the profile is shown on the graph below:

Result from Trine Holm Christensen, @Space, Feb. 2015