* Long curing at 210°C: BCB210AL.PDF/[[file:BCB210BL.PDF|BCB210BL.PDF]]
* Long curing at 210°C: BCB210AL.PDF/[[Media:BCB210BL.PDF|BCB210BL.PDF]]
* Long curing at 250°C: BCB250AL.PDF/[[file:BCB250BL.PDF|BCB250BL.PDF]]
* Long curing at 250°C: BCB250AL.PDF/[[Media:BCB250BL.PDF|BCB250BL.PDF]]


Content of BCB250BL.PDF: (the file BCB210BL.PDF is identical except that the max temperature is 210 instead of 250°C)
Content of BCB250BL.PDF: (the file BCB210BL.PDF is identical except that the max temperature is 210 instead of 250°C)

Revision as of 13:16, 7 September 2017

Feedback to this page: click here

BCB Curing Oven

The BCB Curing Oven. Positioned in the A-4 room

The BCB Curing Oven is mainly used for curing of BCB (bisbenzocyclobutene) and for alloying of metals in a nitrogen atmosphere.

During processing the furnace is rapidly heated by use of eight halogen lamps situated below the sample. The furnace is purged with a high or a low nitrogen flow. Samples are processed at atmospheric pressure or at vacuum.


The user manual, user APV, technical information and contact information can be found in LabManager:

BCB Curing Oven

Process information

Here are some of the standard processes used in the BCB Curing Oven.

BCB curing:

Content of BCB250BL.PDF: (the file BCB210BL.PDF is identical except that the max temperature is 210 instead of 250°C)

;
; stored 31.08.2011  at 17:55:33
{P0}
00,00:30,0020,- - - - 3 - - - -,075,250,001,005,028
01,00:10,0020,- - - 2 - - - - -
02,00:30,0020,- - - - 3 - - - -
03,00:10,0020,- - - 2 - - - - -
04,05:00,0050,H - - 2 - - - - -
05,05:00,0050,H C - 2 - - - - -
06,15:00,0100,H - 1 - - - - - -
07,45:00,0100,H C 1 - - - - - -
08,15:00,0150,H - 1 - - - - - -
09,81:00,0150,H C 1 - - - - - -
10,60:00,0250,H - 1 - - - - - -
11,60:00,0250,H C 1 - - - - - -
12,15:00,0020,- C 1 - - - - - -
13,30:00,0020,- C 1 - - - - - -
14,00:00,0010,- C - - - - - - -

The AL/BL processes are (should be) identical except for a (2x) pump/purge cycle in the beginning of the BL processes.

General processes

There are a number of general processes named DxxxCyyy.PDF.

The Dxxx is the set temperature (in °C) and the Cyyy is the time (in minutes) at the set temperature.

The oven heats to the set temperature (xxx) in 5 mins and then stays at the temperature (xxx) for a time (yyy) after which it cools to room temperature as fast as possible.

The program sequence looks like this for the file D200C060.PDF:

;
; stored 31.08.2011  at 18:15:47
{P0}
00,05:00,0200,H - - 2 - - - - -,075,250,001,005,028
01,60:00,0200,H C 1 - - - - - -
02,05:00,0002,- C 1 - - - - - -
03,00:00,0000,- C - - - - - - -

Equipment performance and process related parameters

Equipment BCB Curing Oven
Purpose
  • BCB curing
  • Metal alloying
Process parameter range Temperature
  • 22 - 450oC
Nitrogen flows
  • Low N2 flow: 5 SLM
  • High N2 flow: Max 16.7 SLM
Pressure
  • Atmospheric pressure or vacuum
Substrates

(Remember to use the right carrier wafer)

Batch size
  • Several small samples
  • One 50 mm wafer
  • One 100 mm wafer
Allowed materials
  • BCB
  • III-V materials
  • Co-polymer
  • Silicon, silicon oxide, silicon nitride
  • Quartz
  • Resist (prebaked)
  • Metal (only Al, Ni, Ge and Au)