Specific Process Knowledge/Lithography/PMMA: Difference between revisions
Appearance
No edit summary |
No edit summary |
||
| Line 26: | Line 26: | ||
| [http://www.allresist.com AllResist] | | [http://www.allresist.com AllResist] | ||
|We have various types of PMMA in the cleanroom. Please contact [mailto:Lithography@danchip.dtu.dk Lithography] for information. | |We have various types of PMMA in the cleanroom. Please contact [mailto:Lithography@danchip.dtu.dk Lithography] for information. | ||
| [[media:MSDS PMMA.pdf|MSDS PMMA]] [[media:AR-P631_679.pdf|Processing guidelines]] | | [[media:MSDS PMMA.pdf|MSDS PMMA]], [[media:AR-P631_679.pdf|Processing guidelines]] | ||
|See table <u>[[Specific_Process_Knowledge/Lithography/Coaters#Coaters:_Comparison_Table|here]] </u> | |See table <u>[[Specific_Process_Knowledge/Lithography/Coaters#Coaters:_Comparison_Table|here]] </u> | ||
|Anisole | |Anisole | ||
|MIBK:IPA (1:3), IPA: | |MIBK:IPA (1:3), H20:IPA (1:3) | ||
|IPA | |IPA | ||
|acetone/1165 | |acetone/1165 | ||
Revision as of 12:19, 2 November 2015
| Resist | Polarity | Manufacturer | Comments | Technical reports | Spinner | Thinner | Developer | Rinse | Remover | Process flows (in docx-format) |
| PMMA | Positive | AllResist | We have various types of PMMA in the cleanroom. Please contact Lithography for information. | MSDS PMMA, Processing guidelines | See table here | Anisole | MIBK:IPA (1:3), H20:IPA (1:3) | IPA | acetone/1165 |
Spin Curves
The thickness is measured on VASE Ellipsometer using a simple Cauchy model for a transparent polymer on Si. The measurements are performed at one incidence angle (70 degrees) only. 9 points on each 4" wafer has been measured; the standard deviation thus representing the homogeinity of the film on the 4" wafers.

| AllResist AR-P 672.03 (PMMA) (~ 2ml per 4" wafer) spin coated on 'Spin Coater: Manual Standard Resists, E-5, WILTID & TIGRE, 26-10-2015. Softbake 3 min @ 150 degC. | ||||||
|---|---|---|---|---|---|---|
| Spin Speed [rpm] | Acceleration [1/s2] | Thickness [nm] | St Dev | |||
| 4000 | 2000 | 95.55 | 0.55 | |||
| 5000 | 2000 | 85.50 | 0.92 | |||
| 7000 | 2000 | 72.79 | 1.18 | |||
| AllResist AR-P 672.03 (PMMA) diluted 1:1 in Anisole (~ 2ml per 4" wafer) spin coated on 'Spin Coater: Manual Standard Resists, E-5, WILTID & TIGRE, 26-10-2015. Softbake 3 min @ 150 degC. | ||||||
|---|---|---|---|---|---|---|
| Spin Speed [rpm] | Acceleration [1/s2] | Thickness [nm] | St Dev | |||
| 2000 | 2000 | 51.37 | 0.25 | |||
| 3000 | 2000 | 41.97 | 0.24 | |||
| 4000 | 2000 | 36.25 | 0.25 | |||
| 5000 | 2000 | 32.42 | 0.30 | |||
| 6000 | 2000 | 30.17 | 0.29 | |||
| 7000 | 2000 | 28.76 | 0.43 | |||