Jump to content

Specific Process Knowledge/Lithography/PMMA: Difference between revisions

From LabAdviser
Tigre (talk | contribs)
Tigre (talk | contribs)
Line 38: Line 38:




[[File:SpinCurvePMMA.jpg|right|400px]]
[[File:SpinCurvePMMA.jpg|right|500px]]
[[:File:SpinCurvePMMA.jpg]]
 


{|border="1" cellspacing="0" cellpadding="3" style="text-align:left;"  style="width: 40%"
{|border="1" cellspacing="0" cellpadding="3" style="text-align:left;"  style="width: 40%"

Revision as of 15:25, 30 October 2015

Resist Polarity Manufacturer Comments Technical reports Spinner Developer Rinse Remover Process flows (in docx-format)
CSAR Positive AllResist Standard positive resist, very similar to ZEP520. Allresist_CSAR62_English.pdf‎,, CSAR_62_Abstract_Allresist.pdf‎ Manual Spinner 1 (Laurell), Spin Coater Labspin XAR-600-546, XAR-600-548, N50, MIBK:IPA IPA AR-600-71, 1165 Remover Process Flow CSAR.docx‎


Spin Curves

The thickness is measured on VASE Ellipsometer using a simple Cauchy model for a transparent polymer on Si. The measurements are performed at one incidence angle (70 degrees) only. 9 points on each 4" wafer has been measured; the standard deviation thus representing the homogeinity of the film on the 4" wafers.



AllResist AR-P 672.03 (PMMA) (~ 2ml per 4" wafer) spin coated on 'Spin Coater: Manual Standard Resists, E-5, WILTID & TIGRE, 26-10-2015. Softbake 3 min @ 150 degC.
Spin Speed [rpm] Acceleration [1/s2] Thickness [nm] St Dev
4000 2000 95.55 0.55
5000 2000 85.50 0.92
7000 2000 72.79 1.18


AllResist AR-P 672.03 (PMMA) diluted 1:1 in Anisole (~ 2ml per 4" wafer) spin coated on 'Spin Coater: Manual Standard Resists, E-5, WILTID & TIGRE, 26-10-2015. Softbake 3 min @ 150 degC.
Spin Speed [rpm] Acceleration [1/s2] Thickness [nm] St Dev
2000 2000 51.37 0.25
3000 2000 41.97 0.24
4000 2000 36.25 0.25
5000 2000 32.42 0.30
6000 2000 30.17 0.29
7000 2000 28.76 0.43