Revision as of 16:48, 16 January 2015
Comparison of continuous processes
| Process | Before (Old showerhead) | After (New showerhead) | |||||
|---|---|---|---|---|---|---|---|
| Name/Type | Description/parameters | Wafer ID | Comment | SEM images | Wafer ID | Comment | SEM images |
| Continuous black silicon recipe on blank wafer | 15 mins, -10 degrees, 32 mtorr, 60 sccm SF6, 55 sccm O2, 70 W platen | S004592 | Wafer centre | S004679 | Wafer centre | ||
| S003900 | Wafer edge | S004679 | Wafer edge | ||||
| Continuous isotropic silicon etch called isoslow7 | 1 minute, 10 degrees, 10 mTorr, 80 SF6, 150 W coil, 3 W platen | S003900 | 4" wafer, 50 % load | S00XXX | No test yet | File:S00XX centre.jpg | |
Comparison of switched processes
Process A
| Recipe | Name | Temp. | Deposition step | Etch step | Comments | |||||||||||||
|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|
| Time | Pres. | C4F8 | SF6 | O2 | Coil | Time | Pres. | C4F8 | SF6 | O2 | Coil | Platen | Showerhead | Runs | Key words | |||
| Process A | Step1 11 cyc | 20 | 4 | 25 | 200 | 0 | 0 | 2000 | 7.0 | 25(1.5s) 90>>150 | 0 | 350(1.5s) 550 | 5 | 2800 | 120>>140(1.5s) 45 | Old | 1 | |
| Step2 44 cyc | 4 | 25 | 200 | 0 | 0 | 2000 | 7.0 | 25(1.5s) 150 | 0 | 350(1.5s) 550 | 5 | 2800 | 140(1.5s) 45 | |||||
| Step1 11 cyc | 20 | 4 | 25 | 200 | 0 | 0 | 2000 | 7.0 | 25(1.5s) 90>>150 | 0 | 350(1.5s) 550 | 5 | 2800 | 120>>140(1.5s) 45 | New | 1 | Profile improved | |
| Step2 44 cyc | 4 | 25 | 200 | 0 | 0 | 2000 | 7.0 | 25(1.5s) 150 | 0 | 350(1.5s) 550 | 5 | 2800 | 140(1.5s) 45 | |||||
SOI
| Recipe | Name | Temp. | Deposition step | Etch step | Comments | |||||||||||||
|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|
| Time | Pres. | C4F8 | SF6 | O2 | Coil | Time | Pres. | C4F8 | SF6 | O2 | Coil | Platen | Showerhead | Runs | Key words | |||
| SOI etch | SOI | 20 | 2 | 25 | 250 | 0 | 0 | 2000 | 3 | 30 | 0 | 400 | 40 | 2800 | 75 (0.025s, 75%) | Old | 1 | |
| SOI | 20 | 2 | 25 | 250 | 0 | 0 | 2000 | 3 | 30 | 0 | 400 | 40 | 2800 | 75 (0.025s, 75%) | New | 1 | OK | |
Process D
| Recipe | Name | Temp. | Deposition step | Etch step | Comments | |||||||||||||
|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|
| Time | Pres. | C4F8 | SF6 | O2 | Coil | Time | Pres. | C4F8 | SF6 | O2 | Coil | Platen | Showerhead | Runs | Key words | |||
| Process D | Original | 0 | 2 | 20 | 150 | 0 | 0 | 2000 | 2.4 | 26 | 0 | 275 | 5 | 2500 | 35 | Old | 1 | |
| Original | 0 | 2 | 20 | 150 | 0 | 0 | 2000 | 2.4 | 26 | 0 | 275 | 5 | 2500 | 35 | New | 1 | ||
| New Process D | 0 | 1 | 20 | 150 | 0 | 0 | 2000 | 3 | 26 | 0 | 275 | 5 | 2500 | 35 | New | 2 | Large undercut | |
| PrD01 | 0 | 1 | 20 | 150 | 0 | 0 | 2000 | 2.4 | 26 | 0 | 275 | 5 | 2500 | 35 | New | 2 | ||
| PrD02 | 0 | 1.1 | 20 | 150 | 0 | 0 | 2000 | 2.4 | 26 | 0 | 275 | 5 | 2500 | 35 | New | 2 | ||
| PrD-3 | 0 | 1 | 20 | 150 | 0 | 0 | 2000 | 2.5 | 26 | 0 | 275 | 5 | 2500 | 35 | New | 2 | ||
| PrD-4 | 0 | 1 | 20 | 150 | 0 | 0 | 2000 | 2.2 | 26 | 0 | 275 | 5 | 2500 | 35 | New | 2 | ||
Polysilicon etch
| Recipe description | Name | Temp. | Deposition step | Etch step | Comments | |||||||||||||
|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|
| Time | Pres. | C4F8 | SF6 | O2 | Coil | Time | Pres. | C4F8 | SF6 | O2 | Coil | Platen | Showerhead | Runs | Key words | |||
| Polysilicon etch | polySi etch DUV mask | 30 | 2.3 | 10 | 50 | 0 | 0 | 600 | 5.0 | 10 | 20 | 60 | 5 | 400 | 40 | Old | 1 | Slightly over-etching to ensure complete absence of grass |
| polySi etch DUV mask | 30 | 2.3 | 10 | 50 | 0 | 0 | 600 | 5.0 | 10 | 20 | 60 | 5 | 400 | 40 | New | 1 | ||
| Cpoly1 | 30 | 1.2 | 10 | 50 | 0 | 0 | 600 | 5.0 | 10 | 20 | 60 | 5 | 400 | 40 | New | 1 | Very aggressive, unusable | |
| Cpoly2 | 30 | 1.4 | 10 | 50 | 0 | 0 | 600 | 5.0 | 10 | 20 | 60 | 5 | 400 | 40 | New | 1 | ||
| Cpoly3 | 30 | 1.6 | 10 | 50 | 0 | 0 | 600 | 5.0 | 10 | 20 | 60 | 5 | 400 | 40 | New | 1 | ||
| Cpoly4 | 30 | 1.8 | 10 | 50 | 0 | 0 | 600 | 5.0 | 10 | 20 | 60 | 5 | 400 | 40 | New | 1 | ||