Specific Process Knowledge/Lithography/LiftOff: Difference between revisions

From LabAdviser
Taran (talk | contribs)
Taran (talk | contribs)
Line 23: Line 23:
|style="background:WhiteSmoke; color:black" align="center"|
|style="background:WhiteSmoke; color:black" align="center"|
NMP (Remover 1165)
NMP (Remover 1165)
|-
!style="background:silver; color:black" align="center" valign="center" rowspan="1"|Performance
|style="background:LightGrey; color:black"|Contact angle
|style="background:WhiteSmoke; color:black" align="center"|
standard recipe 82° (on SiO<sub>2</sub>)
|style="background:WhiteSmoke; color:black" align="center"|
60° - 90°; standard recipe 82° (on SiO<sub>2</sub>)
|-
|-
!style="background:silver; color:black" align="center" valign="center" rowspan="2"|Process parameters
!style="background:silver; color:black" align="center" valign="center" rowspan="2"|Process parameters
Line 43: Line 35:
|style="background:LightGrey; color:black"|Ultrasonic agitation
|style="background:LightGrey; color:black"|Ultrasonic agitation
|style="background:WhiteSmoke; color:black" align="center"|
|style="background:WhiteSmoke; color:black" align="center"|
Yes
Continous
|style="background:WhiteSmoke; color:black" align="center"|
|style="background:WhiteSmoke; color:black" align="center"|
Yes
Continous or pulsed
|-
|-
!style="background:silver; color:black" align="center" valign="center" rowspan="3"|Substrates
!style="background:silver; color:black" align="center" valign="center" rowspan="3"|Substrates

Revision as of 15:24, 5 March 2014

Feedback to this page: click here

Comparing Lift-off equipment

Equipment Lift-off Wet Bench Lift-off (4", 6")
Purpose
  • AZ 5214E lift-off
  • AZ 5214E lift-off
  • AZ nLOF lift-off
Bath chemical

Acetone

NMP (Remover 1165)

Process parameters Process temperature

Room temperature

Heating of the bath is possible.

The heating has been limited to 37°C

Ultrasonic agitation

Continous

Continous or pulsed

Substrates Substrate size
  • 100 mm wafers
  • 100 mm wafers
  • 150 mm wafers
Allowed materials

All cleanroom materials

All cleanroom materials

Batch

1 - 25

1 - 8


Lift-off Wet Bench

Acetone lift-off: positioned in cleanroom 3

This bench is only for wafers with metal!

Here are the main rules for lift-off bench use:

  • Place the wafers in a dedicated wafer holder.
  • Put the holder in the acetone and start the ultrasound. The strip off time is depending of resist thickness.
  • Rinse your wafers for 4-5 min. in running water after stripping.

Find more info about the lift-off process here: Specific Process Knowledge/Photolithography/AZ5214E standard resist - reverse process


Lift-off (4", 6")

bla bla bla