Specific Process Knowledge/Etch/Wet Polysilicon Etch: Difference between revisions

From LabAdviser
Kabi (talk | contribs)
Bghe (talk | contribs)
No edit summary
Line 1: Line 1:
'''Feedback to this page''': '''[mailto:wetchemistry@danchip.dtu.dk?Subject=Feed%20back%20from%20page%20http://labadviser.danchip.dtu.dk/index.php/Specific_Process_Knowledge/Etch/Wet_Polysilicon_Etch click here]'''
'''Feedback to this page''': '''[mailto:labadviser@danchip.dtu.dk?Subject=Feed%20back%20from%20page%20http://labadviser.danchip.dtu.dk/index.php/Specific_Process_Knowledge/Etch/Wet_Polysilicon_Etch click here]'''
 
[[Category: Equipment|Etch Wet Polysilicon]]
[[Category: Etch (Wet) bath|Polysilicon]]


==Wet PolySi Etch==
==Wet PolySi Etch==

Revision as of 14:44, 25 August 2014

Feedback to this page: click here

Wet PolySi Etch

Wet PolySilicon Etch (in the middle): positioned in cleanroom D-3

The wet PolySi Etch is an isotropic silicon etch. This holds for both a poly-silicon thin-film as well as single-crystalline material such as a Si(100) surface. The PolySi Etch process is placed in a dedicated PP-tank in a laminar-flow bench in cleanroom 4.

The PolySi Etch is typically used for opening holes in poly-silicon thin-films, using photoresist as an etch mask. Due to its isotropic nature the under-etching (etch-bias) at least amounts to the thickness of the poly-silicon layer. Another example of usage is etching of "circular-shaped" holes in silicon substrates.

The PolySi Etch is based on the combined oxidation of silicon followed by dissolution of the silicon oxide. The etch solution consists of:

HNO3 : BHF : H2O - (20 : 1 : 20)

NB: The life time of the solution is only a few days.

The user manual and contact information can be found in LabManager:

Isotropic Etch/Poly Etch info page in LabManager

PolySi Etch data

PolySi Etch @ room temperature
General description

Etch of poly-si/Si(100)

Chemical solution HNO3 : BHF : H2O (20 : 1 : 20)
Process temperature Room temperature
Possible masking materials
  • Photoresist(min. 2.2 µm is recommended)
  • LPCVD-oxide (TEOS)
Etch rate
  • RSi ~1000-2000 Å/min (depending on doping level)
  • RSiO2 ~60 Å/min
  • Photoresist (2.2 µm) withstand ~20-30 min
Batch size

1-25 wafers at a time

Size of substrate