At the moment DANCHIP has 3 PECVDs that can deposite silicon oxide with or without dopants of Boron, Phosphorous or Germanium. PECVD1 and PECVD3 are for silicon based processing. PECVD2 is for III-V processing and is described under III-V processing. Look at the [[Specific Process Knowledge/Thin film deposition/PECVD|PECVD]] page to learn more about the PECVDs at DANCHIP. Allthough PECVD1 and PECVD3 are very much alike you cannot count on the a recipe on one system will give exactly the same results on the other system.
At the moment DANCHIP has 2(3) PECVDs that can deposite silicon oxide with or without dopants of Boron, Phosphorous or Germanium. PECVD1 has been decommissioned and PECVD3 are for silicon based processing allowing wafers with small abount of metal (<5% wafer coverage). PECVD2 is clean wafers both for silicon based materials and for III-V materials. At the moment PECVD2 is described under III-V processing. Look at the [[Specific Process Knowledge/Thin film deposition/PECVD|PECVD]] page to learn more about the PECVDs at DANCHIP. All though PECVD2 and PECVD3 are very much alike you cannot count on the a recipe on one system will give exactly the same results on the other system.


=Recipes on PECVD2 for deposition of silicon oxides=
See [[Specific Process Knowledge/III-V Process/thin film dep/pecvd2| here]]


=Recipes on PECVD1 for deposition of silicon oxides=
=Recipes on PECVD1 for deposition of silicon oxides=

Revision as of 08:50, 16 October 2013

Feedback to this page: click here


At the moment DANCHIP has 2(3) PECVDs that can deposite silicon oxide with or without dopants of Boron, Phosphorous or Germanium. PECVD1 has been decommissioned and PECVD3 are for silicon based processing allowing wafers with small abount of metal (<5% wafer coverage). PECVD2 is clean wafers both for silicon based materials and for III-V materials. At the moment PECVD2 is described under III-V processing. Look at the PECVD page to learn more about the PECVDs at DANCHIP. All though PECVD2 and PECVD3 are very much alike you cannot count on the a recipe on one system will give exactly the same results on the other system.

Recipes on PECVD2 for deposition of silicon oxides

See here

Recipes on PECVD1 for deposition of silicon oxides

Recipes

Recipe name SiH4 flow [sccm] N2O flow [sccm] N2 flow [sccm] B2H6 flow [sccm] PH3 flow [sccm] Pressure [mTorr] Power [W] Description
1oxide/1ox_std/standard 17 1600 0 0 0 400 380LF Process control recipe. Developed for waveguides
1PBSG 17 1600 0 135 40 500 800LF Developed for waveguide top cladding by Haiyan Ou @DTU Photonics'.
BGE_PBSG 17 1600 0 240 60 500 800LF Low stress PBSG

Expected results

Recipe name Deposition rate [µm/min] RI Uniformity [%] Comments
1oxide/1ox_std/standard ~0.193 1.46 2 The latest measured values can be seen in the process control sheet in LabManager
1PBSG ~0.3 1.458@633nm

Recipes on PECVD3 for deposition of silicon oxides

Recipes

Recipe name SiH4 flow [sccm] N2O flow [sccm] N2 flow [sccm] B2H6 flow [sccm] PH3 flow [sccm] Pressure [mTorr] Power [W] Description
LFSiO 12 1420 392 0 0 550 60 Uniform silicon oxide
1PBSG 17 1600 0 135 40 500 800LF BPSG glass for waveguide cladding layer

LF=Low Frequency

Expected results

Recipe name Deposition rate [nm/min] RI Uniformity [%]
LFSiO ~75 ~1.48 <1
1PBSG ~228 nm/min . ~17%

Recipes on PECVD3 for deposition of doped oxide

Recipes

Recipe name SiH4 flow [sccm] N2 flow [sccm] GeH4 flow [sccm] (scaled by 100) B2H6 flow [sccm] PH3 flow [sccm] Pressure [mTorr] Power [W] Description
Core-Ge 17 300 300 0 0 400 600 LF Process for germanium doped core layer developed by Haiyan Ou from DTU Photonics

Annnealing: Anneal bond furnace, recipe "core1100"

Top-BPSG 17 0 0 100 40 500 800 LF Process for PBSG top clading layer developed by Haiyan Ou from DTU Photonics

Annnealing/oxidation: Anneal bond furnace, recipe "clad1000"

Expected results

Recipe name Deposition rate [nm/min] Refractive index
Core-Ge ~188 nm/min ~1.46969
Top-BPSG ~248 nm/min ~1.458