Silicon oxide can be etched using either wet chemistry or dry etch equipment. Wet chemistry is mainly used to remove all the oxide on the surface (backside and front side) of a wafer or for isotrotropic etching. Dry etching etches anisotropic. It etches one side of the wafer at a time and can be used to etch structures with several masking materials.
'''Unless anything else is stated, everything on this page, text and pictures are made by DTU Nanolab.'''


Etch of silicon oxide can be done by either wet etch or dry etch. The standard setups for this here at DANCHIP are:
'''All links to Kemibrug (SDS) and Labmanager Including APV and QC requires login.'''
===Wet etches:===
*[[Specific Process Knowledge/Etch/Wet Silicon Oxide Etch (BHF)|Wet Silicon Oxide Etch]]
 
===Dry etches:===
*[[/SiO2 etch using RIE1 or RIE2|Dry etch using RIE1 or RIE2]]
*[[/SiO2 etch using AOE|Dry etch using AOE]]
*[[Specific Process Knowledge/Etch/IBE/IBSD Ionfab 300|IBE/IBSD Ionfab 300]]
 
==Comparison of wet Silicon Oxide etch and dry etches (RIE and AOE) etch for etching of Silicon Oxide==
{| border="2" cellspacing="0" cellpadding="4" align="center"
!
! Wet Silicon Oxide etch (BHF, SIO Etch (wetting agent), 5%HF)
! RIE
! AOE
|- valign="top"
|'''General description'''
|
*Isotropic etch
|
*Anisotropic etch: vertical sidewalls
|
*Anisotropic etch: vertical sidewalls, especially good for deep etch and high aspect ratio etch
|-valign="top"
|'''Possible masking materials'''
|
*Photoresist
*Silicon nitride
|
*Photoresist
*(Poly)Silicon
*Aluminium
*Other metals that covers less the 5% of the wafer area (ONLY RIE2!)
|
*Photoresist
*(Poly)Silicon
*Aluminium
*Chromium (ONLY if the other masking materials can not be used!)
|- valign="top"
|'''Etch rate'''
|
*~75 nm/min (Thermal oxide) in BHF
*~90 nm/min (Thermal oxide) in SIO Etch
*~25 nm/min (Thermal oxide) in 5%HF
|
*Typically 40-120 nm/min can be increased or decreased by using other recipe parameters.
|
*Typically 200-600 nm/min can be increased or decreased by using other recipe parameters.
|-valign="top"
|'''Batch size'''
|
*1-25 wafers at a time
|
*1 wafer at a time
|
*1 wafer at a time
|-valign="top"
|'''Size of substrate'''
|
*4" wafers
|
*4" wafers or smaller pieces
|
*6" or 4" depending on the setup (smaller pieces if you have a carrier wafer)
|-valign="top"
|'''Allowed materials'''
|
*Silicon
*Silicon Oxide
*Silicon Nitride
*Silicon Oxynitride
*Photoresist
*Blue film
*Gold (Au) and Nickel (Ni) (but only in BHF2 (KOH)!)
|
*Silicon
*Silicon Oxide
*Silicon Nitride
*Silicon Oxynitride
*Photoresist
*E-beam resist
*Aluminium
*Other metals that covers less the 5% of the wafer area (ONLY RIE2!)
|
*Silicon
*Silicon Oxide
*Silicon Nitride
*Silicon Oxynitride
*Photoresist
*E-beam resist
*Aluminium
*Chromium (ONLY as masking material if the other masking materials can not be used!)
 
|-
|}


 
'''Feedback to this page''': '''[mailto:labadviser@nanolab.dtu.dk?Subject=Feed%20back%20from%20page%20http://labadviser.nanolab.dtu.dk/index.php/Specific_Process_Knowledge/Etch/Etching_of_Silicon_Oxide click here]'''
 
=This Part is under construction=
 
'''Feedback to this page''': '''[mailto:labadviser@danchip.dtu.dk?Subject=Feed%20back%20from%20page%20http://labadviser.danchip.dtu.dk/index.php/Specific_Process_Knowledge/Etch/Etching_of_Silicon_Nitride click here]'''
<!-- Replace "http://labadviser.danchip.dtu.dk/..." with the link to the Labadviser page-->
<!-- Replace "http://labadviser.danchip.dtu.dk/..." with the link to the Labadviser page-->


== Comparing silicon oxide etch methods at Danchip [[Image:section under construction.jpg|70px]]==
== Comparing silicon oxide etch methods at DTU Nanolab ==
There are a broad varity of silicon oxide etch methods at DTU Nanolab. The methodes are compared here to make it easier for you to compare and choose the one that suits your needs.


There are a broad varity of silicon oxide etch methods at Danchip. The methodes are compared here to make it easier for you to compare and choose the one that suits your needs.
*[[Specific Process Knowledge/Etch/Wet Silicon Oxide Etch (BHF)|Wet Silicon Oxide Etch]]


 
*[[Specific_Process_Knowledge/Etch/III-V_RIE/III_V_RIE_ETCHES#CHF3.2FO2_etch |SiO2 etch using III-V RIE]]
*[[Specific Process Knowledge/Etch/Wet Silicon Nitride Etch|Wet Silicon Nitride Etch]]
*[[/SiO2 etch using AOE|SiO2 etch using AOE]]
*[[/Etch of Silicon Nitride using RIE|Etch of Silicon Nitride using RIE]]
*[[Specific Process Knowledge/Etch/DRIE-Pegasus/Pegasus-4|SiO2 etch with DRIE Pegasus 4]]
*[[Specific Process Knowledge/Etch/AOE (Advanced Oxide Etch)/Silicon Nitride Etch using AOE|Etch of Silicon Nitride using AOE]]
*[[/SiO2 etch using ASE|SiO2 etch using ASE]]
*[[Specific Process Knowledge/Etch/IBE/IBSD Ionfab 300|IBE/Ion Beam Etching using IBSD Ionfab 300]]
*[[Specific_Process_Knowledge/Etch/ICP_Metal_Etcher/silicon_oxide|SiO2 etch using ICP metal]]
*[[Specific Process Knowledge/Etch/IBE&frasl;IBSD Ionfab 300|IBE/IBSD Ionfab 300]]
*[[/SiO2 etch using Plasma Asher|SiO2 etch using Plasma Asher (isotropic)]]


==Compare the methods for Silicon Oxide etching==
==Compare the methods for Silicon Oxide etching==
Line 122: Line 27:
|-style="background:silver; color:black"
|-style="background:silver; color:black"
!
!
![[Specific Process Knowledge/Etch/Wet Silicon Nitride Etch|Wet Silicon Nitride Etch]]
![[Specific Process Knowledge/Etch/Wet Silicon Oxide Etch (BHF)|Wet Silicon Oxide etch (BHF/HF)]]
![[Specific Process Knowledge/Etch/Wet Silicon Oxide Etch (BHF)|BHF]]
![[Specific Process Knowledge/Etch/ASE (Advanced Silicon Etch)|ASE]]
![[Specific Process Knowledge/Etch/RIE (Reactive Ion Etch)|RIE (Reactive Ion Etch)]]
![[Specific Process Knowledge/Etch/III-V RIE |III-V RIE]]
![[Specific Process Knowledge/Etch/AOE (Advanced Oxide Etch)|AOE (Advanced Oxide Etch)]]
![[Specific Process Knowledge/Etch/AOE (Advanced Oxide Etch)|AOE (Advanced Oxide Etch)]]
![[Specific Process Knowledge/Etch/ASE (Advanced Silicon Etch)|ASE (Advanced Silicon Etch)]]
![[Specific Process Knowledge/Etch/DRIE-Pegasus/Pegasus-4|DRIE Pegasus 4]]
![[Specific Process Knowledge/Etch/ICP Metal Etcher|ICP Metal Etch]]
![[Specific Process Knowledge/Etch/ICP Metal Etcher|ICP metal]]
![[Specific Process Knowledge/Etch/IBE&frasl;IBSD Ionfab 300|IBE/IBSD Ionfab 300]]
![[Specific Process Knowledge/Etch/IBE&frasl;IBSD Ionfab 300|IBE/IBSD Ionfab 300]]
![[Specific Process Knowledge/Etch/HF Vapour Phase Etch|HF Vapour Phase Etch]]


|-
|-
Line 137: Line 43:
|
|
*Isotropic etch
*Isotropic etch
*Well suited for removing all nitride on a wafer surface (nitride strip) without a mask. High selectivity Si<sub>3</sub>N<sub>4</sub>/Si (>100) and Si<sub>3</sub>N<sub>4</sub>/SiO<sub>2</sub> (>20) @ 180 C.
|
|
*Isotropic etch
*Anisotropic etch: vertical sidewalls.
*Well suited for removing all  PECVD nitride on a wafer surface (nitride strip) without a mask. Etches LPCVD nitride very slowly
*Primarily for samples with small amounts of metals on.
|
|
*Anisotropic etch: vertical sidewalls
*Anisotropic etch: vertical sidewalls
*Primarily for III-V samples
|
|
*AOE
*Anisotropic etch: vertical sidewalls
|
|
*ASE
*Anisotropic etch: almost vertical sidewalls
|
|
*This is dedicated to metal etch.
*Anisotropic etch: almost vertical sidewalls
*We prefer that SiO2 etch takes place in the AOE or Pegasus 4.
|
|
*Primarily for pure physical etch by sputtering with Ar-ions
*Primarily for pure physical etch by sputtering with Ar-ions
*Also for slanted gratings
|
*Gas phase HF etching with ethanol as carrier
|-
|-


Line 156: Line 66:
|-style="background:LightGrey; color:black"
|-style="background:LightGrey; color:black"
!Possible masking materials
!Possible masking materials
|
*Silicon Oxide
*PolySilicon
|
|
*Photoresist
*Photoresist
*PolySilicon
*PolySilicon
*Silicon nitride (LPCVD)
*Blue film
*Blue film
*Cr/Au for deeper etches (plastic beaker)
|
|
*Photoresist
*Photoresist
*DUV resist
*E-beam resist
*E-beam resist
*Silicon Oxide
*Silicon
*Silicon Nitride
*Silicon Nitride
*Aluminium
*Metals if they cover less than 5% of the wafer area
*Metals if they cover less than 5% of the wafer area (ONLY RIE2!)
|
|
AOE
*Photoresist
*Photoresist and zep resist
*DUV resist
*Silicon Oxide
*E-beam resist
*Aluminum
*Silicon
*Silicon Nitride
*Silicon Nitride
*Aluminium oxide
|
|
ASE
*Photoresist
*Photoresist
*Silicon Oxide
*DUV resist
*E-beam resist
*Silicon
*Silicon Nitride
*Silicon Nitride
*Aluminium
*Aluminium
*Chromium (Please try to avoid this)
|
*Photoresist
*DUV resist
*E-beam resist
*Si
*Silicon Nitride
*Chromium (ask for permission)
|
|
ICP Metal
*Photoresist
*Photo-, DUV- and e-beamresist
*DUV resist
*Silicon Oxide
*E-beam resist
*Si
*Silicon Nitride
*Silicon Nitride
*Aluminium
*Aluminium
*Cr
*Chromium
*Ti
|
|
*Any material that is accepted in the machine
*Any material that is accepted in the machine
|
*Aluminium
*Aluminium oxide
*Polysilicon
|-
|-


Line 198: Line 121:
!Etch rate range
!Etch rate range
|
|
*Si<sub>3</sub>N<sub>4</sub> @ 180 <sup>o</sup>C: ~84 Å/min
*~75 nm/min (Thermal oxide) in BHF
*Si<sub>3</sub>N<sub>4</sub> @ 160 <sup>o</sup>C: ~60 Å/min
*~80 nm/min (Thermal oxide) in BOE 7:1 Etchant VLSI with Surfactant
*~25 nm/min (Thermal oxide) in 5%HF
*~6 nm/min (Thermal oxide) in 1%HF
*~3-4µm/min in 40%HF
|
|
*PECVD nitride: ~400-1000 Å/min
*Process dependent
*Tested range: ~20nm/min - ~250nm/min  
|
|
*Typically 40-50 nm/min can be increased or decreased by using other recipe parameters.
*Process dependent
*Tested range: ~1nm/min - ~30nm/min  
|
|
AOE
*Process dependent
*Tested range: ~60nm/min - ~550nm/min
|
|
ASE
*Process dependent
<500nm/min
|
|
ICP metal
*Process dependent
*Tested range: ~40nm/min - ~200nm/min
|
|
*Process dependant. Has not been tested yet.
*Process dependent
|-
*Tested once ~22nm/min
 
|
*Sample and load dependent
*Expected range: 12 - 175 nm/min
|-
|-
|-style="background:LightGrey; color:black"
|-style="background:LightGrey; color:black"
!Substrate size
!Substrate size
|
*<nowiki>#</nowiki>1-25 100 mm wafers
|
|
*<nowiki>#</nowiki>1-25 100mm wafers in our 100mm bath
*<nowiki>#</nowiki>1-25 100mm wafers in our 100mm bath
*What can be fitted in a plastic beaker
|
|
*As many small samples as can be fitted on the 100mm carrier.
*As many small samples as can be fitted on the 100mm carrier (bad/no cooling!).
*<nowiki>#</nowiki>1 100mm wafer (or smaller with carrier)
*<nowiki>#</nowiki>1 100mm wafer (or smaller with carrier)
*<nowiki>#</nowiki>1 150mm wafer (only when the system is set up for 150mm)  
*<nowiki>#</nowiki>1 150mm wafer (only when set up for 150mm)  
|
|
*As many small samples as can be fitted on a 100mm wafer
*Up to 20cm in diameter
*<nowiki>#</nowiki>1 50 mm wafer fitted on a 100mm wafer
*<nowiki>#</nowiki>1 100 mm wafer
*<nowiki>#</nowiki>1 150 mm wafers (only when the system is set up to 150mm)
|
|
*As many small samples as can be fitted on a 100mm wafer
*As many small samples as can be fitted on a 100mm wafer
Line 235: Line 164:
*<nowiki>#</nowiki>1 100 mm wafer
*<nowiki>#</nowiki>1 100 mm wafer
*<nowiki>#</nowiki>1 150 mm wafers (only when the system is set up to 150mm)
*<nowiki>#</nowiki>1 150 mm wafers (only when the system is set up to 150mm)
|
*As many small samples as can be bonded on a 150mm wafer
*<nowiki>#</nowiki>1 50 mm wafer bonded on a 150mm wafer
*<nowiki>#</nowiki>1 100 mm wafer bonded on a 150nm wafer
*<nowiki>#</nowiki>1 150 mm wafers
|
|
*As many small samples as can be fitted on a 150mm wafer
*As many small samples as can be fitted on a 150mm wafer
*<nowiki>#</nowiki>5 50 mm wafer fitted on a 150mm wafer
*<nowiki>#</nowiki>1 50 mm wafer fittesd on a 150mm wafer
*<nowiki>#</nowiki>1 100 mm wafer on a 150mm wafer
*<nowiki>#</nowiki>1 100 mm wafer fitted on a 150nm wafer
*<nowiki>#</nowiki>1 150 mm wafers (The system is normally set up to 150mm)
*<nowiki>#</nowiki>1 150 mm wafers
|
|
*As many samples as can be securely fitted on a up to 200mm wafer
*As many samples as can be securely fitted on a up to 200mm wafer
Line 246: Line 180:
*<nowiki>#</nowiki>1 150 mm wafers with special carrier
*<nowiki>#</nowiki>1 150 mm wafers with special carrier
*<nowiki>#</nowiki>1 200 mm wafer
*<nowiki>#</nowiki>1 200 mm wafer
|
*Pieces
*<nowiki>#</nowiki>1 50 mm wafer
*<nowiki>#</nowiki>1 100 mm wafer
*<nowiki>#</nowiki>1 150 mm wafer
|-
|-
|-style="background:WhiteSmoke; color:black"
|-style="background:WhiteSmoke; color:black"
!'''Allowed materials'''
!Allowed materials
|
|
In the dedicated bath:
*Silicon
*Silicon
*Silicon Oxide
*Silicon Oxide
*Silicon Nitride
*Silicon Nitride
*Silicon Oxynitride
*Silicon Oxynitride
*Photoresist
*Blue film
In a plastic beaker:
*No limits cross contamination wise
|
|
*[http://labmanager.dtu.dk/function.php?module=XcMachineaction&view=edit&MachID=105 Please take a look in the cross contamination sheet in LabManager for details]
*Silicon
*Silicon
*Silicon Oxide
*Silicon Oxide
Line 260: Line 205:
*Silicon Oxynitride
*Silicon Oxynitride
*Photoresist
*Photoresist
*Blue film
*DUV resist
*E-beam resist
*Other metals if they cover less than 5% of the wafer area
*Quartz/fused silica
|
|
*[http://labmanager.dtu.dk/function.php?module=XcMachineaction&view=edit&MachID=155 Please take a look in the cross contamination sheet in LabManager for details]
*GaAs, GaN, InP, with epitaxial layers
*Aluminum
*Silicon
*Silicon
*Silicon Oxide
*Silicon Oxide
Line 267: Line 218:
*Silicon Oxynitride
*Silicon Oxynitride
*Photoresist
*Photoresist
*DUV resist
*E-beam resist
*E-beam resist
*Other metals if they cover less than 5% of the wafer area (ONLY RIE2!)
*Quartz/fused silica
|
|
*[http://labmanager.dtu.dk/function.php?module=XcMachineaction&view=edit&MachID=115 Please take a look in the cross contamination sheet in LabManager for details]
*Silicon
*Silicon
*Silicon Oxide
*Silicon Oxide
Line 276: Line 227:
*Silicon Oxynitride
*Silicon Oxynitride
*Photoresist
*Photoresist
*zep resist
*DUV resist
*E-beam resist
*Aluminium
*Aluminium
*Chromium (try to avoid it)
*Chromium (try to avoid it)
*Quartz/fused silica
*Quartz/fused silica
|
|
*[http://labmanager.dtu.dk/function.php?module=XcMachineaction&view=edit&MachID=456 Please take a look in the cross contamination sheet in LabManager for details]
*Silicon
*Silicon
*Silicon Oxide
*Silicon Oxide
Line 286: Line 239:
*Silicon Oxynitride
*Silicon Oxynitride
*Photoresist
*Photoresist
*DUV resist
*E-beam resist
*E-beam resist
*Aluminium
*Chromium
*Quartz/fused silica
*Quartz/fused silica
|
|
*[http://labmanager.dtu.dk/function.php?module=XcMachineaction&view=edit&MachID=266 Please take a look in the cross contamination sheet in LabManager for details]
*Silicon
*Silicon
*Photoresist/e-beam resist
*Silicon Oxide
*PolySilicon
*Silicon Nitride
*Silicon oxide
*Silicon Oxynitride
*Silicon (oxy)nitride
*Photoresist
*DUV resist
*E-beam resist
*Aluminium
*Aluminium
*Chromium
*Titanium
*Titanium
*Chromium
*W
*Quartz/fused silica
*Quartz/fused silica
|
|
*[http://labmanager.dtu.dk/function.php?module=XcMachineaction&view=edit&MachID=267 Please take a look in the cross contamination sheet in LabManager for details]
*Silicon
*Silicon
*Silicon oxides
*Silicon oxides
*Silicon (oxy)nitrides
*Silicon (oxy)nitrides
*Metals from the +list
*Metals
*Metals from the -list
*Alloys
*Alloys from the above list
*Stainless steel
*Stainless steel
*Glass
*Glass
Line 312: Line 270:
*Polymers
*Polymers
*Capton tape
*Capton tape
|
*[http://labmanager.dtu.dk/function.php?module=XcMachineaction&view=edit&MachID=458 Please take a look in the cross contamination sheet in LabManager for details]
*Silicon
*Silicon oxides
*Aluminium
|-
|-
|}
|}


<br clear="all" />
<br clear="all" />
==Dry etch with Hard mask==
''By Martin Lind Ommen - ''fall 2016'' '' <br>
Testing selectivities for SiO<sub>2</sub> etching with hard masks on AOE and ICP metal with different recipes.All tests are done with 100% etching load<br>
[[File:Dry etching by Martin Lind Ommen Fall 2016.png|600px]]<br>
MLO_psi is the version of SiO2_psi on labadviser that is shown under low line with reduction.<br>
The recipe ICP is on ICP metal call: A SiO2 etch with C4F8 with resist mask<br>
I had problems with this recipe - it gave polymer on the surface, therefor I do not have more info on that.<br>

Latest revision as of 15:45, 28 March 2025

Unless anything else is stated, everything on this page, text and pictures are made by DTU Nanolab.

All links to Kemibrug (SDS) and Labmanager Including APV and QC requires login.

Feedback to this page: click here

Comparing silicon oxide etch methods at DTU Nanolab

There are a broad varity of silicon oxide etch methods at DTU Nanolab. The methodes are compared here to make it easier for you to compare and choose the one that suits your needs.

Compare the methods for Silicon Oxide etching

Wet Silicon Oxide etch (BHF/HF) ASE III-V RIE AOE (Advanced Oxide Etch) DRIE Pegasus 4 ICP metal IBE/IBSD Ionfab 300 HF Vapour Phase Etch
Generel description
  • Isotropic etch
  • Anisotropic etch: vertical sidewalls.
  • Primarily for samples with small amounts of metals on.
  • Anisotropic etch: vertical sidewalls
  • Primarily for III-V samples
  • Anisotropic etch: vertical sidewalls
  • Anisotropic etch: almost vertical sidewalls
  • Anisotropic etch: almost vertical sidewalls
  • We prefer that SiO2 etch takes place in the AOE or Pegasus 4.
  • Primarily for pure physical etch by sputtering with Ar-ions
  • Also for slanted gratings
  • Gas phase HF etching with ethanol as carrier
Possible masking materials
  • Photoresist
  • PolySilicon
  • Silicon nitride (LPCVD)
  • Blue film
  • Cr/Au for deeper etches (plastic beaker)
  • Photoresist
  • DUV resist
  • E-beam resist
  • Silicon
  • Silicon Nitride
  • Metals if they cover less than 5% of the wafer area
  • Photoresist
  • DUV resist
  • E-beam resist
  • Aluminum
  • Silicon
  • Silicon Nitride
  • Photoresist
  • DUV resist
  • E-beam resist
  • Silicon
  • Silicon Nitride
  • Aluminium
  • Chromium (Please try to avoid this)
  • Photoresist
  • DUV resist
  • E-beam resist
  • Si
  • Silicon Nitride
  • Chromium (ask for permission)
  • Photoresist
  • DUV resist
  • E-beam resist
  • Si
  • Silicon Nitride
  • Aluminium
  • Chromium
  • Any material that is accepted in the machine
  • Aluminium
  • Aluminium oxide
  • Polysilicon
Etch rate range
  • ~75 nm/min (Thermal oxide) in BHF
  • ~80 nm/min (Thermal oxide) in BOE 7:1 Etchant VLSI with Surfactant
  • ~25 nm/min (Thermal oxide) in 5%HF
  • ~6 nm/min (Thermal oxide) in 1%HF
  • ~3-4µm/min in 40%HF
  • Process dependent
  • Tested range: ~20nm/min - ~250nm/min
  • Process dependent
  • Tested range: ~1nm/min - ~30nm/min
  • Process dependent
  • Tested range: ~60nm/min - ~550nm/min
  • Process dependent

<500nm/min

  • Process dependent
  • Tested range: ~40nm/min - ~200nm/min
  • Process dependent
  • Tested once ~22nm/min
  • Sample and load dependent
  • Expected range: 12 - 175 nm/min
Substrate size
  • #1-25 100mm wafers in our 100mm bath
  • What can be fitted in a plastic beaker
  • As many small samples as can be fitted on the 100mm carrier (bad/no cooling!).
  • #1 100mm wafer (or smaller with carrier)
  • #1 150mm wafer (only when set up for 150mm)
  • Up to 20cm in diameter
  • As many small samples as can be fitted on a 100mm wafer
  • #1 50 mm wafer fitted on a 100mm wafer
  • #1 100 mm wafer
  • #1 150 mm wafers (only when the system is set up to 150mm)
  • As many small samples as can be bonded on a 150mm wafer
  • #1 50 mm wafer bonded on a 150mm wafer
  • #1 100 mm wafer bonded on a 150nm wafer
  • #1 150 mm wafers
  • As many small samples as can be fitted on a 150mm wafer
  • #1 50 mm wafer fittesd on a 150mm wafer
  • #1 100 mm wafer fitted on a 150nm wafer
  • #1 150 mm wafers
  • As many samples as can be securely fitted on a up to 200mm wafer
  • #1 50 mm wafer with special carrier
  • #1 100 mm wafer with special carrier
  • #1 150 mm wafers with special carrier
  • #1 200 mm wafer
  • Pieces
  • #1 50 mm wafer
  • #1 100 mm wafer
  • #1 150 mm wafer
Allowed materials

In the dedicated bath:

  • Silicon
  • Silicon Oxide
  • Silicon Nitride
  • Silicon Oxynitride
  • Photoresist
  • Blue film

In a plastic beaker:

  • No limits cross contamination wise


Dry etch with Hard mask

By Martin Lind Ommen - fall 2016
Testing selectivities for SiO2 etching with hard masks on AOE and ICP metal with different recipes.All tests are done with 100% etching load

MLO_psi is the version of SiO2_psi on labadviser that is shown under low line with reduction.
The recipe ICP is on ICP metal call: A SiO2 etch with C4F8 with resist mask
I had problems with this recipe - it gave polymer on the surface, therefor I do not have more info on that.