Specific Process Knowledge/Etch/ICP Metal Etcher/silicon/nano/Sinano3: Difference between revisions
Appearance
Created page with "== The Sinano3.0 recipe == {| border="2" cellpadding="2" cellspacing="1" |+ '''Recipe Sinano3.0''' |- ! rowspan="6" align="center"| Recipe | Gas | BCl<sub>3</sub> 5 sccm, HB..." |
No edit summary |
||
| (4 intermediate revisions by the same user not shown) | |||
| Line 1: | Line 1: | ||
<!-- Ok, jmli 20170627 --> | |||
<!-- Ok, jmli 2020-0120 --> | |||
<!-- Page reviewed 9/8-2022 jmli --> | |||
<!--Checked for updates on 4/4-2025 - ok/jmli --> | |||
== The Sinano3.0 recipe == | == The Sinano3.0 recipe == | ||
<!-- revised 1/6-2015 by jmli --> | |||
{| border="2" cellpadding="2" cellspacing="1" | {| border="2" cellpadding="2" cellspacing="1" | ||
|+ '''Recipe Sinano3.0''' | |+ '''Recipe Sinano3.0''' | ||
| Line 75: | Line 80: | ||
|- | |- | ||
|} | |} | ||
== The Sinano3.0 recipe == | == The Sinano3.0 recipe == | ||
Latest revision as of 07:41, 4 April 2025
The Sinano3.0 recipe
| Recipe | Gas | BCl3 5 sccm, HBr 15 sccm |
|---|---|---|
| Pressure | 2 mTorr, Strike 3 secs @ 5 mTorr | |
| Power | 900 W CP, 50 W PP | |
| Temperature | 20 degs | |
| Hardware | 100 mm Spacers | |
| Time | 150 secs | |
| Conditions | Run ID | 417, 418 and 419 |
| Conditioning | Sequence: Oxygen clean, MU tests, processes, no oxygen between runs | |
| Mask | 110 nm zep etched down to 64 nm | |
| Wafer | WF_2A#4_feb06_2011 |
- The results of the Sinano3.0 recipe
-
The 30 nm trenches
-
The 60 nm trenches
-
The 90 nm trenches
-
The 120 nm trenches
-
The 150 nm trenches
| Nominal trench line width | ' | ' | 30 | 60 | 90 | 120 | 150 | Average | Std. dev. |
| Etch rate | nm/min | 236 | 307 | 333 | 341 | 339 | 311 | 44 | |
| Sidewall angle | degs | 84 | 82 | 83 | 81 | 80 | 82 | 2 | |
| CD loss | nm/edge | 28 | 46 | 62 | 88 | 103 | 65 | 30 | |
| CD loss foot | nm/edge | 28 | 46 | 62 | 88 | 103 | 65 | 30 | |
| Bowing | 21 | 32 | 35 | 33 | 36 | 31 | 6 | ||
| Bottom curvature | -30 | -27 | -18 | 14 | 16 | -9 | 22 | ||
| Zep etch rate | 46 |
The Sinano3.0 recipe
| Recipe | Gas | BCl3 5 sccm, HBr 15 sccm |
|---|---|---|
| Pressure | 2 mTorr, Strike 3 secs @ 5 mTorr | |
| Power | 900 W CP, 50 W PP | |
| Temperature | 20 degs | |
| Hardware | 100 mm Spacers | |
| Time | 150 secs | |
| Conditions | Run ID | 417, 418 and 419 |
| Conditioning | Sequence: Oxygen clean, MU tests, processes, no oxygen between runs | |
| Mask | 110 nm zep etched down to 64 nm | |
| Wafer | WF_2A#4_feb06_2011 |
- The results of the Sinano3.0 recipe
-
The 30 nm trenches
-
The 60 nm trenches
-
The 90 nm trenches
-
The 120 nm trenches
-
The 150 nm trenches
| Nominal trench line width | ' | ' | 30 | 60 | 90 | 120 | 150 | Average | Std. dev. |
| Etch rate | nm/min | 236 | 307 | 333 | 341 | 339 | 311 | 44 | |
| Sidewall angle | degs | 84 | 82 | 83 | 81 | 80 | 82 | 2 | |
| CD loss | nm/edge | 28 | 46 | 62 | 88 | 103 | 65 | 30 | |
| CD loss foot | nm/edge | 28 | 46 | 62 | 88 | 103 | 65 | 30 | |
| Bowing | 21 | 32 | 35 | 33 | 36 | 31 | 6 | ||
| Bottom curvature | -30 | -27 | -18 | 14 | 16 | -9 | 22 | ||
| Zep etch rate | 46 |