Jump to content

Specific Process Knowledge/Lithography/Strip/plasmaAsher05: Difference between revisions

From LabAdviser
Jehem (talk | contribs)
Jehem (talk | contribs)
 
(5 intermediate revisions by the same user not shown)
Line 32: Line 32:


==Process development sections==
==Process development sections==
*[[Specific Process Knowledge/Lithography/Strip/plasmaAsher04_processDevelopment|Process development for plasma asher 04 and plasma asher 05]]
*[[Specific Process Knowledge/Lithography/Strip/plasmaAsher04_processDevelopment|Stripping with plasma asher 4 and plasma asher 5]]
*[[Specific Process Knowledge/Etch/Etching of Silicon Oxide/SiO2 etch using Plasma Asher |SiO<sub>2</sub> etch using Plasma Asher 1]]
*[[Specific Process Knowledge/Lithography/Descum/plasmaAsher05|Descumming with plasma asher 4 and plasma asher 5]]
*[[Specific Process Knowledge/Lithography/Descum/plasmaAsher05|Descum using plasma asher 5]]
*[[Specific Process Knowledge/Etch/Etching of Silicon Oxide/SiO2 etch using Plasma Asher |CF<sub>4</sub> etch of SiO<sub>2</sub> in Plasma Asher 1]]
<br clear="all" />
<br clear="all" />

Latest revision as of 09:55, 25 June 2026

Plasma Asher 5

Plasma asher 5 in cleanroom E-5.

Product name: PVA Tepla Gigabatch 380M
Year of purchase: 2024

The Plasma Asher 5 can be used for the following processes:

  • Photoresist stripping
  • Descumming
  • Surface cleaning
  • Removal of organic passivation layers and masks


Furthermore plasma processing using CF4 in plasma asher 5 can be used for:

  • Etching of glass and ceramic
  • Etching of SiO2, Si3N4, Si
  • Removal of polyimide layers


Plasma asher 5 can be used for almost every material, but if you have any doubt if your materials are compatible/allowed in plasma asher 5, feel free to ask the lithography group at Nanolab.

The user manual, risk assessment, and contact information can be found in LabManager - requires login

Process Information

Typical stripping parameters
Tested with 1.5 µm AZ 5214E on 100 mm silicon substrate.

  • O2: 100 sccm
  • N2: 100 sccm
  • Pressure (DSC): 1.3 mbar
  • Power: 1000 W
  • Time (single wafer): 20-30 minutes
  • Time (full boat): 90 minutes