Specific Process Knowledge/Lithography/Aligners/MAvsMLA: Difference between revisions
Appearance
m →Yield |
|||
| (3 intermediate revisions by the same user not shown) | |||
| Line 24: | Line 24: | ||
===Yield=== | ===Yield=== | ||
The yield is measured by inspecting all 116 lithographic resolution test structures in an optical microscope and recording the smallest resolved dots and lines. | |||
<br clear="all" /> | <br clear="all" /> | ||
| Line 81: | Line 77: | ||
'''Effect of WEC pressure for mask aligner (after WEC head service):''' | '''Effect of WEC pressure for mask aligner (after WEC head service):''' | ||
{| cellpadding="2" style="border: 2px solid darkgray;" align="center" | |||
! width="460" | | |||
! width="460" | | |||
|+'''Wafer maps at different WEC pressure for Aligner: MA6-2 (Dose 100mJ/cm<sup>2</sup>)''' | |||
|- border="0" align="center" | |||
|[[Image:Map_MA6-2_soft_WEC015.jpg|450px]] | |||
|[[Image:Map_MA6-2_soft_WEC040.jpg|450px]] | |||
|- align="center" | |||
| Soft contact, 0.15bar WEC pressure. <br/>Resolution: 3.92µm average; 0.9µm standard deviation. <br/>Yield at 2.5µm: 8% || Soft contact, 0.40bar WEC pressure. <br/>Resolution: 2.19µm average; 0.5µm standard deviation. <br/>Yield at 2.5µm: 86% | |||
|- border="0" align="center" | |||
|[[Image:Map_MA6-2_prox_WEC015.jpg|450px]] | |||
|[[Image:Map_MA6-2_prox_WEC040.jpg|450px]] | |||
|- align="center" | |||
| 10µm proximity, 0.15bar WEC pressure. <br/>Resolution: 3.22µm average; 0.8µm standard deviation. <br/>Yield at 2.5µm: 34% || 10µm proximity, 0.40bar WEC pressure. <br/>Resolution: 2.83µm average; 0.6µm standard deviation. <br/>Yield at 2.5µm: 66% | |||
|} | |||
<br clear="all" /> | |||
===Resist profile (sidewall angle and linewidth)=== | ===Resist profile (sidewall angle and linewidth)=== | ||
Latest revision as of 15:55, 11 June 2026
The content on this page, including all images and pictures, was created by DTU Nanolab staff, unless otherwise stated.
Feedback to this page: click here
Mask Aligner vs Maskless Aligner
Slides presented at NNUM in Uppsala 2026: MA6 vs MLA 2026_v09
Mask design used in the investigation: LithoTestAlign_2025_v10.gds
Additional data
THIS PAGE IS UNDER CONSTRUCTION
AZ 5214E
Resolution
- Table with optimal parameters and resolution for different aligners
- SEM pictures
Yield
The yield is measured by inspecting all 116 lithographic resolution test structures in an optical microscope and recording the smallest resolved dots and lines.
Effect of exposure mode for mask aligner:
Effect of WEC pressure for mask aligner (after WEC head service):
Resist profile (sidewall angle and linewidth)
- SEM pictures to support graphs?

Blue circles: Exposed on Aligner: MA6-2 in vacuum contact.
Orange Squares: Exposed on Aligner: Maskless 02 (MLA2) using defoc 2 (QC defoc=2).

Blue circles: Exposed on Aligner: MA6-2 in vacuum contact.
Orange Squares: Exposed on Aligner: Maskless 02 (MLA2) using defoc 2 (QC defoc=2).

Blue circles: Width of 2µm line. Orange Squares: Sidewall angle.
AZ MiR 701
Resolution
- Table with optimal parameters and resolution for different aligners
- SEM pictures
Resist profile (sidewall angle and linewidth)
- SEM pictures to support graphs?

Blue circles: Exposed on Aligner: MA6-2 in vacuum contact.
Orange Squares: Exposed on Aligner: Maskless 02 (MLA2) using defoc 2 (QC defoc=2).

Blue circles: Exposed on Aligner: MA6-2 in vacuum contact.
Orange Squares: Exposed on Aligner: Maskless 02 (MLA2) using defoc 2 (QC defoc=2).

Blue circles: Width of 2µm line. Orange Squares: Sidewall angle.
AZ nLOF 2020
Resolution
- Table with optimal parameters and resolution for different aligners
- SEM pictures
Resist profile (sidewall angle and linewidth)
- SEM pictures to support graphs?

Blue circles: Exposed on Aligner: MA6-2 in vacuum contact.
Orange Squares: Exposed on Aligner: Maskless 01 (MLA1) using defoc -4 (QC defoc=-2).
Grey triangles: Exposed on Aligner: Maskless 02 (MLA2) using defoc 0 (QC defoc=2).

Blue circles: Exposed on Aligner: MA6-2 in vacuum contact.
Orange Squares: Exposed on Aligner: Maskless 01 (MLA1) using defoc -4 (QC defoc=-2).
Grey triangles: Exposed on Aligner: Maskless 02 (MLA2) using defoc 0 (QC defoc=2).

Blue circles: Width of 2µm line. Orange Squares: Sidewall angle.

Blue circles: Width of 2µm line. Orange Squares: Sidewall angle.