=Developer: TMAH Manual 02=
=Developer: TMAH Manual 02=
[[file:Developer_TMAH_manual_02.jpg|400px|right|thumb|Developer: TMAH Manual 02 is located in E-4.]]
[[file:Developer_TMAH_manual_02.jpg|400px|right|thumb|Developer: TMAH Manual 02 is located in E-4.]]


Developer: TMAH Manual 02 is a manually operated puddle developer for single wafers or chips. The wafers or chips are loaded manually one by one into the developer, but the developer dispense, puddle time, water rinse, and drying is performed automatically.  
'''Tool description'''<br>
The Developer: TMAH manual 02 is a semi-automatic and programmable single substrate developer system, which can be used for development of resists on chips, 50 mm, 100 mm and 150 mm substrates. The development is done using AZ 726 MIF, which is a 2.38% TMAH solution with wetting agent.
 
Single substrates are loaded manually into the tool, but the developer dispense, puddle time, agitation, rinse and drying is controlled by the tool.


The development uses the TMAH based AZ 726 MIF developer (2.38 % TMAH in water with a small amount of wetting agent).
{| class="wikitable"
! style="text-align:left" | Product
| style="padding-left: 10px" | Laurell EDC-650-HZB-23NP
|-
! style="text-align:left" | Year of purchase
| style="padding-left: 10px" | 2016
|-
! style="text-align:left" | Tool modification
| style="padding-left: 10px" |
Converted from e-beam solvent developer to UV TMAH developer in 2024<br>
Added media flow controllers for developer, rinse and drying media in 2025
|-
! style="text-align:left" | Location
| style="padding-left: 10px" | Cleanroom E-4
|}


'''[https://www.youtube.com/watch?v=btinNzYnLnY Training video]'''
'''User manual'''<br>
The user manual and contact information can be found in [http://labmanager.dtu.dk/function.php?module=Machine&view=view&mach=341 LabManager] - '''requires login'''
 
'''Tool training'''<br>
Training on the tool requires users to complete the [https://labadviser.nanolab.dtu.dk//index.php?title=Specific_Process_Knowledge/Lithography#Lithography_Tool_Package_Training lithography TPT] followed by the online tool training and a hands-on authorization training.<br>
The tool training video is part of the online tool training, but can also be viewed [https://www.youtube.com/watch?v=btinNzYnLnY here].
<br clear="all" />
 
=Equipment performance and process related parameters=
{| class="wikitable"
|-
! scope=row style="text-align: left;" | Tool purpose
|
Development of UV resists:
*AZ nLOF 2020
*AZ MIR 701
*AZ 5214E
*AZ 4562
Development of DUV resists:
*KrF M230Y
*KrF M35G
|-
! scope=row style="text-align: left;" | Developer
| AZ 726 MIF (2.38% TMAH)
|-
! scope=row style="text-align: left;" | Development method
| Puddle
|-
! scope=row style="text-align: left;" | Handling method
|
*Non-vacuum chuck for 100 mm & 150 mm wafers
*Non-vacuum chuck for chips and 50 mm wafers
|-
! scope=row style="text-align: left;" | Process temperature
| Room temperature
|-
! scope=row style="text-align: left;" | Process agitaion
| 15 cycles per minute
|-
! scope=row style="text-align: left;" | Process rinse
| DI water
|-
! scope=row style="text-align: left;" | Substrate sizes
|
*Chips
*50 mm wafers
*100 mm wafers
*150 mm wafers
|-
! scope=row style="text-align: left;" | Substrate materials
|
*All cleanroom allowed materials
*Film, or pattern, of all materials except Type IV
|-
! scope=row style="text-align: left;" | Substrate batch size
| 1
|}
<br clear="all" />


The user manual, user APV, and contact information can be found in [http://labmanager.dtu.dk/function.php?module=Machine&view=view&mach=324 LabManager] - '''requires login'''


=Process information=
=Process information=
All recipes use the following structure:
All recipes use the following structure:
#Pressurize the TMAH canister
#Pressurize the TMAH canister
#Pre-wet substrate at high RPM
#Dispense puddle while rotating substrate slowly
#Dispense puddle while rotating substrate slowly
#Puddle development with agitation of substrate
#Puddle development with agitation of substrate
Line 19: Line 95:
#Dry substrate and chamber with nitrogen
#Dry substrate and chamber with nitrogen


Multipuddle recipes repeat steps 2-4 for the given number of puddles.


'''Multi puddle'''<br>
Multi puddle recipes repeat steps 2-4 for the given number of puddles.


==Process recipes==
==Process recipes==
Line 36: Line 113:


Tests were performed on under-exposed resist, specifically for showing the difference between the agitation and non-agitation puddle development - the measured results cannot necessarily be transferred directly to a working process, only the vague general behavior of the two process setups; faster/slower development speed and better/worse uniformity across substrate.
Tests were performed on under-exposed resist, specifically for showing the difference between the agitation and non-agitation puddle development - the measured results cannot necessarily be transferred directly to a working process, only the vague general behavior of the two process setups; faster/slower development speed and better/worse uniformity across substrate.
[[file:ManualTMAHdeveloper developRate v1.png|400px|thumb|Development rate for under-exposed resist test]]
[[file:ManualTMAHdeveloper uniformity v1.png|400px|thumb|Non-uniformity for under-exposed resist test]]


{| class="wikitable"
{| class="wikitable"
Line 44: Line 124:
|  
|  
*Slower development
*Slower development
*Higher non-uniformity
*Worse uniformity
|
|
*Faster development
*Faster development
Line 54: Line 134:
! scope=row style="text-align: left;" | Non-uniformity
! scope=row style="text-align: left;" | Non-uniformity
| 21% || 11%
| 21% || 11%
|-
! scope=row style="text-align: left;" | Agitation
| None || 15 cycles per minute, 20 rpm, 500 rpm/s
|-
|-
! scope=row style="text-align: left;" | Substrate
! scope=row style="text-align: left;" | Substrate
| colspan="2"|100 mm SSP silicon
| colspan="2"|100 mm SSP silicon
|-
|-
! scope=row style="text-align: left;" | Resist
! scope=row style="text-align: left;" | Resist film
| colspan="2"|AZ 5214E
| colspan="2"|1.5 µm AZ 5214E
|-
|-
! scope=row style="text-align: left;" | Exposure dose
! scope=row style="text-align: left;" | Exposure dose
Line 70: Line 153:
| colspan="2"|AZ 726 MIF (2.38% TMAH)
| colspan="2"|AZ 726 MIF (2.38% TMAH)
|}
|}
<br clear="all" />
<br clear="all"/>
 
<gallery style="text-align: center;" widths=450 heights=350>
ManualTMAHdeveloper developRate v1.png|Development rate for under-exposed resist test
ManualTMAHdeveloper uniformity v1.png|Non-uniformity for under-exposed resist test
</gallery>
 
=Equipment performance and process related parameters=
 
{| class="wikitable"
|-
! scope=row style="text-align: left;" | Tool purpose
|
Development of UV resists:
*AZ nLOF 2020
*AZ MIR 701
*AZ 5214E
*AZ 4562
Development of DUV resists:
*KrF M230Y
*KrF M35G
|-
! scope=row style="text-align: left;" | Developer
|
AZ 726 MIF (2.38% TMAH)
|-
! scope=row style="text-align: left;" | Development method
| Puddle
|-
! scope=row style="text-align: left;" | Handling method
|
*Non-vacuum chuck for 100 mm & 150 mm wafers
*Non-vacuum chuck for chips and 50 mm wafers
|-
! scope=row style="text-align: left;" | Process temperature
| Room temperature
|-
! scope=row style="text-align: left;" | Process agitaion
| 15 cycles per minute
|-
! scope=row style="text-align: left;" | Process rinse
| DI water
|-
! scope=row style="text-align: left;" | Substrate sizes
|
*Chips
*50 mm wafers
*100 mm wafers
*150 mm wafers
|-
! scope=row style="text-align: left;" | Substrate materials
|
*All cleanroom allowed materials
*Film, or pattern, of all materials except Type IV
|-
! scope=row style="text-align: left;" | Substrate batch size
| 1
|}
<br clear="all" />

Latest revision as of 15:17, 18 February 2026

The content on this page, including all images and pictures, was created by DTU Nanolab staff, unless otherwise stated.

Developer: TMAH Manual 02

Developer: TMAH Manual 02 is located in E-4.

Tool description
The Developer: TMAH manual 02 is a semi-automatic and programmable single substrate developer system, which can be used for development of resists on chips, 50 mm, 100 mm and 150 mm substrates. The development is done using AZ 726 MIF, which is a 2.38% TMAH solution with wetting agent.

Single substrates are loaded manually into the tool, but the developer dispense, puddle time, agitation, rinse and drying is controlled by the tool.

Product Laurell EDC-650-HZB-23NP
Year of purchase 2016
Tool modification

Converted from e-beam solvent developer to UV TMAH developer in 2024
Added media flow controllers for developer, rinse and drying media in 2025

Location Cleanroom E-4

User manual
The user manual and contact information can be found in LabManager - requires login

Tool training
Training on the tool requires users to complete the lithography TPT followed by the online tool training and a hands-on authorization training.
The tool training video is part of the online tool training, but can also be viewed here.

Equipment performance and process related parameters

Tool purpose

Development of UV resists:

  • AZ nLOF 2020
  • AZ MIR 701
  • AZ 5214E
  • AZ 4562

Development of DUV resists:

  • KrF M230Y
  • KrF M35G
Developer AZ 726 MIF (2.38% TMAH)
Development method Puddle
Handling method
  • Non-vacuum chuck for 100 mm & 150 mm wafers
  • Non-vacuum chuck for chips and 50 mm wafers
Process temperature Room temperature
Process agitaion 15 cycles per minute
Process rinse DI water
Substrate sizes
  • Chips
  • 50 mm wafers
  • 100 mm wafers
  • 150 mm wafers
Substrate materials
  • All cleanroom allowed materials
  • Film, or pattern, of all materials except Type IV
Substrate batch size 1



Process information

All recipes use the following structure:

  1. Pressurize the TMAH canister
  2. Pre-wet substrate at high RPM
  3. Dispense puddle while rotating substrate slowly
  4. Puddle development with agitation of substrate
  5. Spin off developer
  6. Clean substrate and chamber with DI water
  7. Dry substrate and chamber with nitrogen


Multi puddle
Multi puddle recipes repeat steps 2-4 for the given number of puddles.

Process recipes

(Updated 2026-01-12, JEHEM)

  • -Rinse-
  • 1x015s
  • 1x030s
  • 1x060s
  • 1x120s
  • 2x060s
  • 5x060s

Agitation

Testing showed that adding agitation to the puddle step gave better uniformity in the development rate over the entire area of the substrate as well as increased development rate.

Tests were performed on under-exposed resist, specifically for showing the difference between the agitation and non-agitation puddle development - the measured results cannot necessarily be transferred directly to a working process, only the vague general behavior of the two process setups; faster/slower development speed and better/worse uniformity across substrate.

Development rate for under-exposed resist test
Non-uniformity for under-exposed resist test
Non-agitation Agitation
Test results
  • Slower development
  • Worse uniformity
  • Faster development
  • Better uniformity
Normalized development rate 1 1.20
Non-uniformity 21% 11%
Agitation None 15 cycles per minute, 20 rpm, 500 rpm/s
Substrate 100 mm SSP silicon
Resist film 1.5 µm AZ 5214E
Exposure dose 50 mJ/cm2 (~50% of normal dose)
Development Single puddle for 60 seconds
Developer AZ 726 MIF (2.38% TMAH)