Jump to content

Specific Process Knowledge/Etch/DRIE-Pegasus/nanoetch/nano141: Difference between revisions

From LabAdviser
Jml (talk | contribs)
Jmli (talk | contribs)
No edit summary
 
(5 intermediate revisions by the same user not shown)
Line 1: Line 1:
'''Feedback to this page''': '''[mailto:labadviser@nanolab.dtu.dk?Subject=Feed%20back%20from%20page%20http://labadviser.nanolab.dtu.dk/index.php/Specific_Process_Knowledge/Etch/DRIE-Pegasus/nanoetch/nano141 click here]'''
<!--Checked for updates on 30/7-2018 - ok/jmli -->
<!--Checked for updates on 5/10-2020 - ok/jmli -->
<!--Checked for updates on 4/9-2025 - ok/jmli -->
== The nano1.41 recipe ==
== The nano1.41 recipe ==
{{Template:Author-jmli1}}
<!--Checked for updates on 2/02-2023 - ok/jmli -->


{| border="2" cellpadding="2" cellspacing="1"  
{| border="2" cellpadding="2" cellspacing="1"  

Latest revision as of 10:26, 4 September 2025

Feedback to this page: click here

The nano1.41 recipe

Unless otherwise stated, all content on this page was created by Jonas Michael-Lindhard, DTU Nanolab

Recipe nano1.41
Recipe Gas C4F8 75 sccm, SF6 38 sccm
Pressure 4 mTorr, Strike 3 secs @ 15 mTorr
Power 800 W CP, 75 W PP
Temperature -20 degs
Hardware 100 mm Spacers
Time 120 secs
Conditions Run ID 2001
Conditioning Sequence: Oxygen clean, MU tests, processes, no oxygen between runs
Mask 211 nm zep etched down to 10 nm



Nominal trench line width ' 30 60 90 120 150 Average Std. dev.
Etch rates nm/min 155 161 164 171 179 166 9
Sidewall angle degs 91 90 90 90 90 90 1
CD loss nm/edge -1 -11 -13 -36 -37 -20 16
CD loss foot nm/edge 4 1 0 -22 -10 -5 11
Bowing 5 2 5 4 1 3 2
Bottom curvature -45 -40 -34 -29 -23 -34 9
zep nm/min 101