Specific Process Knowledge/Etch/DRIE-Pegasus/nanoetch/nano143: Difference between revisions
Appearance
New page: == The nano1.43 recipe == {| border="2" cellpadding="2" cellspacing="1" |+ '''Recipe nano1.43''' |- ! rowspan="6" align="center"| Recipe | Gas | C<sub>4</sub>F<sub>8</sub> 75 sccm, SF<su... |
No edit summary |
||
| (6 intermediate revisions by 2 users not shown) | |||
| Line 1: | Line 1: | ||
'''Feedback to this page''': '''[mailto:labadviser@nanolab.dtu.dk?Subject=Feed%20back%20from%20page%20http://labadviser.nanolab.dtu.dk/index.php/Specific_Process_Knowledge/Etch/DRIE-Pegasus/nanoetch/nano143 click here]''' | |||
<!--Checked for updates on 30/7-2018 - ok/jmli --> | |||
<!--Checked for updates on 5/10-2020 - ok/jmli --> | |||
<!--Checked for updates on 4/9-2025 - ok/jmli --> | |||
== The nano1.43 recipe == | == The nano1.43 recipe == | ||
{{Template:Author-jmli1}} | |||
<!--Checked for updates on 2/02-2023 - ok/jmli --> | |||
{| border="2" cellpadding="2" cellspacing="1" | {| border="2" cellpadding="2" cellspacing="1" | ||
| Line 44: | Line 51: | ||
C4F8 75 sccm, SF6 38 sccm, 4 mTorr, Strike 3 secs @ 15 mTorr, 800 W CP, 30 W PP, -20 degs, 120 secs | C4F8 75 sccm, SF6 38 sccm, 4 mTorr, Strike 3 secs @ 15 mTorr, 800 W CP, 30 W PP, -20 degs, 120 secs | ||
</gallery> | </gallery> | ||
{| {{table}} | |||
| align="center" style="background:#f0f0f0;"|'''Nominal trench line width''' | |||
| align="center" style="background:#f0f0f0;"|'''''' | |||
| align="center" style="background:#f0f0f0;"|'''30''' | |||
| align="center" style="background:#f0f0f0;"|'''60''' | |||
| align="center" style="background:#f0f0f0;"|'''90''' | |||
| align="center" style="background:#f0f0f0;"|'''120''' | |||
| align="center" style="background:#f0f0f0;"|'''150''' | |||
| align="center" style="background:#f0f0f0;"|'''Average''' | |||
| align="center" style="background:#f0f0f0;"|'''Std. dev.''' | |||
|- | |||
| Etch rates||nm/min||139||147||149||152||152||148||6 | |||
|- | |||
| Sidewall angle||degs||90||90||90||90||90||90||0 | |||
|- | |||
| CD loss||nm/edge||6||-21||-21||-41||-45||-24||21 | |||
|- | |||
| CD loss foot||nm/edge||11||-8||-8||-28||-18||-10||14 | |||
|- | |||
| Bowing||||1||-1||1||1||0||0||1 | |||
|- | |||
| Bottom curvature||||-50||-47||-34||-32||-31||-39||9 | |||
|- | |||
| zep||nm/min||||||||||||55|| | |||
|- | |||
| | |||
|} | |||
Latest revision as of 10:26, 4 September 2025
Feedback to this page: click here
The nano1.43 recipe
Unless otherwise stated, all content on this page was created by Jonas Michael-Lindhard, DTU Nanolab
| Recipe | Gas | C4F8 75 sccm, SF6 38 sccm |
|---|---|---|
| Pressure | 4 mTorr, Strike 3 secs @ 15 mTorr | |
| Power | 800 W CP, 30 W PP | |
| Temperature | -20 degs | |
| Hardware | 100 mm Spacers | |
| Time | 120 secs | |
| Conditions | Run ID | 2018 |
| Conditioning | Sequence: Oxygen clean, MU tests, processes, no oxygen between runs | |
| Mask | 211 nm zep etched down to 102 nm |
- The results of the nano1.43 recipe
-
The 30 nm trenches
-
The 60 nm trenches
-
The 90 nm trenches
-
The 120 nm trenches
-
The 150 nm trenches
| Nominal trench line width | ' | 30 | 60 | 90 | 120 | 150 | Average | Std. dev. |
| Etch rates | nm/min | 139 | 147 | 149 | 152 | 152 | 148 | 6 |
| Sidewall angle | degs | 90 | 90 | 90 | 90 | 90 | 90 | 0 |
| CD loss | nm/edge | 6 | -21 | -21 | -41 | -45 | -24 | 21 |
| CD loss foot | nm/edge | 11 | -8 | -8 | -28 | -18 | -10 | 14 |
| Bowing | 1 | -1 | 1 | 1 | 0 | 0 | 1 | |
| Bottom curvature | -50 | -47 | -34 | -32 | -31 | -39 | 9 | |
| zep | nm/min | 55 | ||||||