!Generel description | !Generel description | ||
| | | | ||
*Evaporation of Ti pellets in the presence of | *Evaporation of Ti or Ti<sub>2</sub>O<sub>3</sub> pellets in the presence of O<sub>2</sub>. | ||
*Can heat up to 250 °C. | |||
| | | | ||
*Reactive DC sputtering of Ti target | *Reactive DC sputtering of Ti target | ||
| Line 35: | Line 36: | ||
*Reactive pulsed DC sputtering | *Reactive pulsed DC sputtering | ||
*Reactive HIPIMS (high-power impulse magnetron sputtering) | *Reactive HIPIMS (high-power impulse magnetron sputtering) | ||
*Can heat up to 6000 °C | |||
| | | | ||
*Reactive DC sputtering of Ti target in Ar/O<sub>2</sub> (10 % O<sub>2</sub>) plasma | *Reactive DC sputtering of Ti target in Ar/O<sub>2</sub> (10 % O<sub>2</sub>) plasma | ||
| Line 40: | Line 42: | ||
| | | | ||
*ALD (atomic layer deposition) of TiO<sub>2</sub> | *ALD (atomic layer deposition) of TiO<sub>2</sub> | ||
*Can heat up to 350 °C | |||
|- | |- | ||
|- | |- | ||
|-style="background:LightGrey; color:black" | |-style="background:LightGrey; color:black" | ||
!Stoichiometry | !Stoichiometry and form | ||
| | | | ||
*Can probably be varied, expect somewhat O-poor composition | *Can probably be varied, expect somewhat O-poor composition | ||
| Line 111: | Line 114: | ||
!More info on TiO2 | !More info on TiO2 | ||
| | | | ||
* | *Expect lower density than bulk material of same stoichiometry. | ||
| | | | ||
*[[Specific Process Knowledge/Thin film deposition/TiO2 deposition using Sputter-System Metal-Oxide(PC1)|TiO2 deposition using Sputter-System Metal-Oxide(PC1)]] | *[[Specific Process Knowledge/Thin film deposition/TiO2 deposition using Sputter-System Metal-Oxide(PC1)|TiO2 deposition using Sputter-System Metal-Oxide(PC1)]] | ||