Specific Process Knowledge/Lithography/MiR: Difference between revisions
No edit summary |
|||
| (4 intermediate revisions by 2 users not shown) | |||
| Line 1: | Line 1: | ||
{{ | {{cc-nanolab}} | ||
'''Feedback to this page''': '''[mailto:labadviser@nanolab.dtu.dk?Subject=Feed%20back%20from%20page%20http://labadviser.nanolab.dtu.dk/index.php/Specific_Process_Knowledge/Lithography/MiR click here]''' | '''Feedback to this page''': '''[mailto:labadviser@nanolab.dtu.dk?Subject=Feed%20back%20from%20page%20http://labadviser.nanolab.dtu.dk/index.php/Specific_Process_Knowledge/Lithography/MiR click here]''' | ||
| Line 21: | Line 21: | ||
==Exposure== | ==Exposure== | ||
'''Dehydration of resist film:'''<br> | '''Dehydration of resist film:'''<br> | ||
During exposure in the maskless aligners, MiR can be sensitive to dehydration by the air flow applied by the pneumatic auto-focus mechanism. This may lead to insufficient development, especially for small substrates. This problem can be alleviated by switching to the overview camera for a period of 1 minute before starting the exposure, or simply by parking the writehead away from the exposure location for 1 minute before starting the exposure. | During exposure in the maskless aligners, MiR can be sensitive to dehydration by the air flow applied by the pneumatic auto-focus mechanism. This may lead to insufficient development, especially for small substrates. This problem can be alleviated by switching to the overview camera for a period of 1 minute before starting the exposure, or simply by parking the writehead away from the exposure location for 1 minute before starting the exposure. Dehydration can also mess up a dose test, but this can be fixed by increasing the spacing between the individual doses, or even better by extending the test design to 40mm or more in the Y-direction (adding a very small structure in the design file, or increasing the upper boarder during conversion). | ||
The effect can also be reduced by increasing the soft bake. | The effect can also be reduced by increasing the soft bake. | ||
| Line 31: | Line 31: | ||
During exposure, interaction between the incoming light and the light reflected by the substrate can cause a standing wave to form in the resist (especially true for single line/wavelength exposure). This leads to a wavy sidewall after development. The standing wave pattern can be | During exposure, interaction between the incoming light and the light reflected by the substrate can cause a standing wave to form in the resist (especially true for single line/wavelength exposure). This leads to a wavy sidewall after development. The standing wave pattern can be reduced by introducing a post-exposure bake before development, which allows the activated PAC to diffuse into un-activated regions, thus smoothing the sidewall. The recommended PEB for MiR is 60 s at 110°C (for a 1 - 2 µm film). Thicker coatings may require longer bake, and substrate thickness and material may also affect the required baking time. | ||
Since the post-exposure bake is at an elevated temperature compared to the soft bake, it will cause the resist film to become 5-10% thinner (probably due to continued evaporation of solvent). A 1. | Since the post-exposure bake is at an elevated temperature compared to the soft bake, it will cause the resist film to become 5-10% thinner (probably due to continued evaporation of solvent). A 1.5 µm thick MiR resist film will be approximately 1.4 µm after PEB. | ||
<gallery style="text-align: center;" widths=450 heights=350> | |||
MIR_noPEB.jpg|1.5 µm AZ MIR 701 without PEB | |||
MIR_withPEB.jpg|1.5 µm AZ MIR 701 with PEB | |||
</gallery> | |||
==Development== | ==Development== | ||
'''Development speed:''' | '''Development speed:''' | ||
*Puddle development in 2.38% TMAH (AZ 726 MIF): ~2 µm/min | *Puddle development in 2.38% TMAH (AZ 726 MIF): ~2 µm/min | ||
Latest revision as of 13:39, 5 May 2026
The content on this page, including all images and pictures, was created by DTU Nanolab staff, unless otherwise stated.
Feedback to this page: click here
Resist description
AZ MiR 701 is a positive UV photoresist. It is considered to have high selectivity for dry etching.
Spin coating
Typical spin parameters:
- Spin off: 30-60 s
- Soft bake: 60 s @ 90°C in proximity
Exposure
Dehydration of resist film:
During exposure in the maskless aligners, MiR can be sensitive to dehydration by the air flow applied by the pneumatic auto-focus mechanism. This may lead to insufficient development, especially for small substrates. This problem can be alleviated by switching to the overview camera for a period of 1 minute before starting the exposure, or simply by parking the writehead away from the exposure location for 1 minute before starting the exposure. Dehydration can also mess up a dose test, but this can be fixed by increasing the spacing between the individual doses, or even better by extending the test design to 40mm or more in the Y-direction (adding a very small structure in the design file, or increasing the upper boarder during conversion).
The effect can also be reduced by increasing the soft bake.
Post-exposure bake
Typical PEB parameters:
- PEB temperature: 110°C
- PEB time: 60 s
During exposure, interaction between the incoming light and the light reflected by the substrate can cause a standing wave to form in the resist (especially true for single line/wavelength exposure). This leads to a wavy sidewall after development. The standing wave pattern can be reduced by introducing a post-exposure bake before development, which allows the activated PAC to diffuse into un-activated regions, thus smoothing the sidewall. The recommended PEB for MiR is 60 s at 110°C (for a 1 - 2 µm film). Thicker coatings may require longer bake, and substrate thickness and material may also affect the required baking time.
Since the post-exposure bake is at an elevated temperature compared to the soft bake, it will cause the resist film to become 5-10% thinner (probably due to continued evaporation of solvent). A 1.5 µm thick MiR resist film will be approximately 1.4 µm after PEB.
-
1.5 µm AZ MIR 701 without PEB
-
1.5 µm AZ MIR 701 with PEB
Development
Development speed:
- Puddle development in 2.38% TMAH (AZ 726 MIF): ~2 µm/min