Jump to content

Specific Process Knowledge/Lithography/5214E: Difference between revisions

From LabAdviser
Jehem (talk | contribs)
Jehem (talk | contribs)
No edit summary
 
(10 intermediate revisions by 2 users not shown)
Line 1: Line 1:
{{cc-nanolab}}
'''Feedback to this page''': '''[mailto:labadviser@nanolab.dtu.dk?Subject=Feed%20back%20from%20page%20http://labadviser.nanolab.dtu.dk/index.php/Specific_Process_Knowledge/Lithography/5214E click here]'''
[[Category: Lithography|Resist]]
[[Category: Resist|AZ 5214E]]
__TOC__
__TOC__


Line 5: Line 12:


==Spin coating==
==Spin coating==
[[Image:5214Espincurves.JPG|500x500px|thumb|Spin curves for AZ 5214E using a 30 s spin-off, and a 60s @ 90°C softbake]]
[[Image:5214Espincurves.JPG|500x500px|thumb|Spin curves for AZ 5214E (old German version) using a 30 s spin-off, and a 60s @ 90°C softbake]]


'''Typical spin parameters:'''
'''Typical spin parameters:'''
*Spin off: 30-60 s
*Spin off: 30-60 s
*Soft bake: 60s @ 90°C
*Soft bake: 60 s @ 90°C


<br clear="all" />
<br clear="all" />


==Image reversal==
==Image reversal==
If 5214E is baked after exposure, the exposed resist will cross-link, making it insoluble in the developer. This is called the "Reversal bake", or sometimes the post-exposure bake. The reversal bake activates cross-linking of the exposed areas, which "reverses" the polarity of the design.
'''Typical image reversal parameters:'''
*Reversal bake temperature: 110°C
*Reversal bake time: 60 s
*Flood exposure: 500 mJ/cm<sup>2</sup>
 


If the substrate is flood exposed after the reversal bake, the previously unexposed areas become soluble, and will be removed in the subsequent development. The reversal procedure effectively makes AZ 5214E a negative resist.
If 5214E is baked after exposure, the exposed resist will cross-link, making it insoluble in the developer. This is called the "Reversal bake". The reversal bake activates cross-linking of the exposed areas, which "reverses" the polarity of the design. When the substrate is flood-exposed after the reversal bake, the previously unexposed areas become soluble, and will be removed in the subsequent development. The image reversal procedure effectively makes AZ 5214E a negative resist.


The image reversal process greatly increases the sensitivity of AZ 5214E, and the dose of the image exposure is a critical parameter, especially if negative angled resist sidewalls are desired.<br>
The image reversal process greatly increases the sensitivity of AZ 5214E, and the dose of the image exposure is a critical parameter, especially if negative angled resist sidewalls are desired. In coatings below 2 µm, it is difficult to achieve undercut.<br>
Half dose of the normal, positive process is a good starting point for optimization. Similarly, the reversal bake is also a critical step, and must be tightly controlled in order to achieve consistent results. If negative sidewalls are desired, 60-120s at 110°C is recommended (as well as a resist thickness above 2 µm), but if straight sidewalls are desired, 60-120s at 120°C can be used.  
Half dose of the normal, positive process is a good starting point for optimization. Similarly, the reversal bake is also a critical step, and must be tightly controlled in order to achieve consistent results. If negative sidewalls are desired, 60 - 120 s at 110°C is recommended (as well as a resist thickness above 2 µm), but if straight sidewalls are desired, 60 - 120 s at 120°C can be used.  


The flood exposure, on the other hand, is uncritical, and 2-5 times the normal positive process dose is generally used.
The flood exposure, on the other hand, is uncritical, and ~5 times the normal positive process dose is generally used.


==Development==
==Development==
'''Development speed:'''
'''Development speed:'''
*Puddle development in 2.38% TMAH (AZ 726 MIF): ~2 µm/min
*Puddle development in 2.38% TMAH (AZ 726 MIF): ~2 µm/min

Latest revision as of 12:25, 20 April 2026

The content on this page, including all images and pictures, was created by DTU Nanolab staff, unless otherwise stated.

Feedback to this page: click here

Resist description

AZ 5214E is a positive UV photoresist with image reversal capability. It is considered to have good adhesion when wet etching.

Spin coating

Spin curves for AZ 5214E (old German version) using a 30 s spin-off, and a 60s @ 90°C softbake

Typical spin parameters:

  • Spin off: 30-60 s
  • Soft bake: 60 s @ 90°C


Image reversal

Typical image reversal parameters:

  • Reversal bake temperature: 110°C
  • Reversal bake time: 60 s
  • Flood exposure: 500 mJ/cm2


If 5214E is baked after exposure, the exposed resist will cross-link, making it insoluble in the developer. This is called the "Reversal bake". The reversal bake activates cross-linking of the exposed areas, which "reverses" the polarity of the design. When the substrate is flood-exposed after the reversal bake, the previously unexposed areas become soluble, and will be removed in the subsequent development. The image reversal procedure effectively makes AZ 5214E a negative resist.

The image reversal process greatly increases the sensitivity of AZ 5214E, and the dose of the image exposure is a critical parameter, especially if negative angled resist sidewalls are desired. In coatings below 2 µm, it is difficult to achieve undercut.
Half dose of the normal, positive process is a good starting point for optimization. Similarly, the reversal bake is also a critical step, and must be tightly controlled in order to achieve consistent results. If negative sidewalls are desired, 60 - 120 s at 110°C is recommended (as well as a resist thickness above 2 µm), but if straight sidewalls are desired, 60 - 120 s at 120°C can be used.

The flood exposure, on the other hand, is uncritical, and ~5 times the normal positive process dose is generally used.

Development

Development speed:

  • Puddle development in 2.38% TMAH (AZ 726 MIF): ~2 µm/min