Specific Process Knowledge/Thin film deposition/Deposition of Aluminium: Difference between revisions
| (39 intermediate revisions by 2 users not shown) | |||
| Line 1: | Line 1: | ||
'''Feedback to this page''': '''[mailto:labadviser@nanolab.dtu.dk?Subject=Feed%20back%20from%20page%20http://labadviser.nanolab.dtu.dk/index.php/Specific_Process_Knowledge/Thin_film_deposition/Deposition_of_Aluminium click here]''' | |||
<i> Unless otherwise stated, this page is written by <b>DTU Nanolab internal</b></i> | |||
< | |||
<br clear="all" /> | <br clear="all" /> | ||
== Deposition of Aluminium == | == Deposition of Aluminium == | ||
Aluminium can be deposited by e-beam evaporation, | Aluminium can be deposited by e-beam evaporation, sputtering and thermal evaporation. In the chart below we compare the different methods and available equipment. | ||
==Sputtering of Aluminium== | ==Sputtering of Aluminium== | ||
Aluminium may be sputter deposited in either | Aluminium may be sputter deposited in either the single-chamber sputter-system ("Sputter System Lesker") or the cluster-based sputter system ("Sputter-System Metal-Oxide(PC1)" and "Sputter-System Metal-Nitride(PC3)"). See more in links here and the chart below. | ||
*[[/Sputter | *[[Specific Process Knowledge/Thin film deposition/Deposition of Aluminium/Al sputtering in Sputter System (Lesker)|Al sputtering in Sputter System (Lesker)]] | ||
*[[Specific Process Knowledge/Thin film deposition/Deposition of Aluminium/Al Sputtering in Cluster Lesker PC3|Al Sputtering in Sputter-System Metal-Nitride(PC3)]] | |||
==E-beam evaporation of Aluminium== | ==E-beam evaporation of Aluminium== | ||
Aluminium can be deposited by e-beam assisted evaporation in the | Aluminium can be deposited by e-beam assisted evaporation in the two Temescal e-beam evaporators. | ||
*[[/Al Ebeam evaporation in Temescal |E-beam evaporation of Al in Temescal]] | *[[/Al Ebeam evaporation in Temescal |E-beam evaporation of Al in Temescal]] | ||
*[[/Notes on low oxygen content in e-beam prepared Al thin films|Notes on low oxygen content in e-beam prepared Al thin films (Temescal)]] | |||
<!----> | <!----> | ||
==Thermal deposition of Aluminium== | ==Thermal deposition of Aluminium== | ||
In the | In the Lesker Thermal evaporator aluminium can be deposited by thermal deposition. Some properties of the evaporated films are described on the following page: | ||
*[[/Thermal deposition of Al|Thermal deposition of Aluminium]] | *[[/Thermal deposition of Al|Thermal deposition of Aluminium]] | ||
==Comparison of Al deposition options== | |||
<br clear="all" /> | <br clear="all" /> | ||
{|border="1" cellspacing="1" cellpadding="3" style="text-align:left;" | {|border="1" cellspacing="1" cellpadding="3" style="text-align:left;" | ||
|- | |- | ||
|- | |- | ||
|-style="background:silver; color:black" | |-style="background:silver; color:black" | ||
| Line 42: | Line 41: | ||
! | ! | ||
! E-beam evaporation ([[Specific Process Knowledge/Thin film deposition/Temescal|Temescal]]) | ! E-beam evaporation ([[Specific Process Knowledge/Thin film deposition/Temescal|E-beam evaporator (Temescal)]]) | ||
! E-beam evaporation ([[Specific Process Knowledge/Thin film deposition/ | ! E-beam evaporation ([[Specific Process Knowledge/Thin film deposition/10-pocket e-beam evaporator|E-beam evaporator (10-pockets)]]) | ||
! Sputter deposition ([[Specific Process Knowledge/Thin film deposition/Lesker|Sputter-System (Lesker)]]) | |||
! Sputter deposition ([[Specific Process Knowledge/Thin film deposition/ | ! Sputter deposition ([[Specific Process Knowledge/Thin film deposition/Cluster-based multi-chamber high vacuum sputtering deposition system|Sputter-system Metal-Oxide (PC1) and Sputter-system Metal-Nitride (PC3)]]) | ||
! | |||
! Thermal evaporation ([[Specific Process Knowledge/Thin film deposition/thermalevaporator|Thermal Evaporator]]) | ! Thermal evaporation ([[Specific Process Knowledge/Thin film deposition/thermalevaporator|Thermal Evaporator]]) | ||
|- | |- | ||
| Line 53: | Line 51: | ||
| | | | ||
E-beam deposition of Aluminium | E-beam deposition of Aluminium. Option to tilt substrate. | ||
| | | | ||
E-beam deposition of Aluminium | E-beam deposition of Aluminium. Option to tilt substrate. | ||
| | | | ||
Sputter deposition of Aluminium | Sputter deposition of Aluminium (DC) | ||
| | | | ||
Sputter deposition of Aluminium (DC, Pulsed DC, HIPIMS) | |||
| | | | ||
Aluminum deposition onto unexposed e-beam resist | Aluminum deposition onto unexposed e-beam resist | ||
| Line 68: | Line 64: | ||
! Pre-clean | ! Pre-clean | ||
|Ar ion etch | |Ar ion etch | ||
| | | | ||
| | | | ||
|RF Ar clean | |RF Ar clean | ||
| | | | ||
|- | |- | ||
|-style="background:WhiteSmoke; color:black" | |-style="background:WhiteSmoke; color:black" | ||
! Layer thickness | ! Layer thickness | ||
|10Å to 1 µm* | |10Å to 1 µm* | ||
|10Å to 1 µm* | |10Å to 1 µm* | ||
|10Å to ~0.5µm (very time consuming ) | |10Å to ~0.5µm (very time consuming ) | ||
|10Å to 0. | |10Å to ~0.5µm | ||
|10Å to 1 µm | |10Å to 1 µm* | ||
|- | |- | ||
|-style="background:LightGrey; color:black" | |-style="background:LightGrey; color:black" | ||
! Deposition rate | ! Deposition rate | ||
| | |1Å/s to 10Å/s | ||
| | |1Å/s to 5Å/s | ||
|Depending on [[/Al sputtering in Sputter System (Lesker) |process parameters]] at least up to 0.7 Å/s | |||
|Depending on [[/Sputter | |Depending on process parameters at least up to 1.3 Å/s. See conditions [[Specific_Process_Knowledge/Thin_film_deposition/Cluster-based_multi-chamber_high_vacuum_sputtering_deposition_system#Standard_recipe_performance|here]] | ||
| | |||
|0.5, 1, or 2 Å/s | |0.5, 1, or 2 Å/s | ||
|- | |- | ||
| Line 98: | Line 91: | ||
*smaller pieces | *smaller pieces | ||
| | | | ||
*Up to | *Up to 4x6" or 3x8" wafers | ||
*smaller pieces | *smaller pieces | ||
| | | | ||
* | *1x4" wafer or | ||
* | *1x6" wafer or | ||
several small samples | |||
| | | | ||
* | *up to 10x4" wafers or | ||
* | *up to 10x6" wafers | ||
* | *or many smaller samples | ||
| | | | ||
* | *Up to 3 x 4" wafers or one 6" or 8" wafer (limited uniformity on large substrates) | ||
*Many small chips | |||
|-style="background:LightGrey; color:black" | |-style="background:LightGrey; color:black" | ||
| Line 119: | Line 109: | ||
| | | | ||
Approx. 20 min | Approx. 20-30 min | ||
| | | | ||
Approx. 20-30 min | |||
| | |||
Approx. 10 min | Approx. 10 min | ||
| | | | ||
Approx. | Approx. 5 min plus 6 min transfer time | ||
| | | | ||
Approx. 15-20 min | |||
Approx. 15 min | |||
|-style="background:WhiteSmoke; color:black" | |-style="background:WhiteSmoke; color:black" | ||
! Allowed | ! Allowed materials | ||
| | | | ||
Almost any that does not degas. See the [http://labmanager.dtu.dk/function.php?module=XcMachineaction&view=edit&MachID=429 cross-contamination sheet]. | |||
| | | | ||
Almost any that does not degas. See the [http://labmanager.dtu.dk/function.php?module=XcMachineaction&view=edit&MachID=511 cross-contamination sheet]. | |||
| | | | ||
* Silicon wafers | * Silicon wafers | ||
* | * and almost any | ||
| | | | ||
* | *Almost that does not degas - see cross contamination sheets for [http://labmanager.dtu.dk/function.php?module=XcMachineaction&view=edit&MachID=441 PC1] and [http://labmanager.dtu.dk/function.php?module=XcMachineaction&view=edit&MachID=442 PC3] | ||
* Special carrier for III-V materials. | |||
* | |||
| | | | ||
Almost any that does not degas. See the [http://labmanager.dtu.dk/function.php?module=XcMachineaction&view=edit&MachID=404 cross-contamination sheet]. | |||
|} | |} | ||
'''*''' ''For | '''*''' ''For cumulative deposition above 600 nm please write to metal@nanolab.dtu.dk to make sure there will be enough Al for your deposition'' | ||
==Aluminium deposition on ZEP520A for lift-off - comparison of thermal and e-beam evaporation == | ==Aluminium deposition on ZEP520A for lift-off - comparison of thermal and e-beam evaporation == | ||
| Line 256: | Line 148: | ||
==Aluminium deposition on AZ5214 for lift-off== | ==Aluminium deposition on AZ5214 for lift-off== | ||
Negative photolithography process is | Negative photolithography process is recommended. | ||
Positive photolithography process from 1.5 µm is possible especially for thin layers of metal. | |||
The more pattern the easier the lift-off. | |||
It was tried (jan09) to lift 2.5 µm Al on 4.2 µm negative resist on top of 11 µm APOX SiO2 in an acetone sonic-bath. | |||
The Al deposition was done in steps evaporating 500 nm a time with 5 min pause and pressure down to at least 2 E-6 mbar before proceeding. | |||
Latest revision as of 07:14, 18 June 2025
Feedback to this page: click here
Unless otherwise stated, this page is written by DTU Nanolab internal
Deposition of Aluminium
Aluminium can be deposited by e-beam evaporation, sputtering and thermal evaporation. In the chart below we compare the different methods and available equipment.
Sputtering of Aluminium
Aluminium may be sputter deposited in either the single-chamber sputter-system ("Sputter System Lesker") or the cluster-based sputter system ("Sputter-System Metal-Oxide(PC1)" and "Sputter-System Metal-Nitride(PC3)"). See more in links here and the chart below.
E-beam evaporation of Aluminium
Aluminium can be deposited by e-beam assisted evaporation in the two Temescal e-beam evaporators.
Thermal deposition of Aluminium
In the Lesker Thermal evaporator aluminium can be deposited by thermal deposition. Some properties of the evaporated films are described on the following page:
Comparison of Al deposition options
| E-beam evaporation (E-beam evaporator (Temescal)) | E-beam evaporation (E-beam evaporator (10-pockets)) | Sputter deposition (Sputter-System (Lesker)) | Sputter deposition (Sputter-system Metal-Oxide (PC1) and Sputter-system Metal-Nitride (PC3)) | Thermal evaporation (Thermal Evaporator) | |
|---|---|---|---|---|---|
| General description |
E-beam deposition of Aluminium. Option to tilt substrate. |
E-beam deposition of Aluminium. Option to tilt substrate. |
Sputter deposition of Aluminium (DC) |
Sputter deposition of Aluminium (DC, Pulsed DC, HIPIMS) |
Aluminum deposition onto unexposed e-beam resist |
| Pre-clean | Ar ion etch | RF Ar clean | |||
| Layer thickness | 10Å to 1 µm* | 10Å to 1 µm* | 10Å to ~0.5µm (very time consuming ) | 10Å to ~0.5µm | 10Å to 1 µm* |
| Deposition rate | 1Å/s to 10Å/s | 1Å/s to 5Å/s | Depending on process parameters at least up to 0.7 Å/s | Depending on process parameters at least up to 1.3 Å/s. See conditions here | 0.5, 1, or 2 Å/s |
| Batch size |
|
|
several small samples |
|
|
| Pumping time from wafer load |
Approx. 20-30 min |
Approx. 20-30 min |
Approx. 10 min |
Approx. 5 min plus 6 min transfer time |
Approx. 15-20 min |
| Allowed materials |
Almost any that does not degas. See the cross-contamination sheet. |
Almost any that does not degas. See the cross-contamination sheet. |
|
Almost any that does not degas. See the cross-contamination sheet. |
* For cumulative deposition above 600 nm please write to metal@nanolab.dtu.dk to make sure there will be enough Al for your deposition
Aluminium deposition on ZEP520A for lift-off - comparison of thermal and e-beam evaporation
This is a small study of which aluminium deposition that is best for aluminium lift-off on ZEP520A resist and a very thin layer of aluminium (~20nm). The grain size is compared for the different methods.
The conclusion was that e-beam evaporation of aluminium at 15 Å/s gave the best result.
See details of the study here.
Aluminium deposition on AZ5214 for lift-off
Negative photolithography process is recommended.
Positive photolithography process from 1.5 µm is possible especially for thin layers of metal.
The more pattern the easier the lift-off.
It was tried (jan09) to lift 2.5 µm Al on 4.2 µm negative resist on top of 11 µm APOX SiO2 in an acetone sonic-bath. The Al deposition was done in steps evaporating 500 nm a time with 5 min pause and pressure down to at least 2 E-6 mbar before proceeding.