Jump to content

Specific Process Knowledge/Etch/ICP Metal Etcher/silicon/nano/Sinano34: Difference between revisions

From LabAdviser
Jmli (talk | contribs)
No edit summary
Jmli (talk | contribs)
No edit summary
 
(One intermediate revision by the same user not shown)
Line 1: Line 1:
<!--Checked for updates on 10/7-2019 - ok/jmli -->
<!--Checked for updates on 10/7-2019 - ok/jmli -->
<!-- Ok, jmli 20170627 -->
<!-- Ok, jmli 20170627 -->
<!--Checked for updates on 24/8-2021. ok/ jmli-->
<!--Checked for updates on 4/4-2025 - ok/jmli -->
== The Sinano3.4 recipe ==
== The Sinano3.4 recipe ==
<!-- revised 1/6-2015 by jmli -->
<!-- revised 1/6-2015 by jmli -->

Latest revision as of 08:36, 4 April 2025


The Sinano3.4 recipe

Recipe Sinano3.4
Recipe Gas BCl3 5 sccm, HBR 15 sccm
Pressure 2 mTorr, Strike 3 secs @ 5 mTorr
Power 900 W CP, 90 W PP
Temperature 20 degs
Hardware 100 mm Spacers
Time 120 secs
Conditions Run ID 431 ID
Conditioning Sequence: Oxygen clean, MU tests, processes, no oxygen between runs
Mask The 180 nm zep resist etched down to 72 nm


Nominal trench line width ' ' 30 60 90 120 150 Average Std. dev.
Etch rate nm/min 78 114 125 129 133 116 22
Sidewall angle degs 83,07278187 82,82949277 81,35457747 80,01059257 80,6398092 82 1
CD loss nm/edge -13 -11 -12 -12 -5 -11 3
CD loss foot nm/edge -13 -2 3 6 15 2 10
Bowing 9 8 6 6 -1 5 4
Bottom curvature -22 -10 -6 -4 -6 -9 7
Zep etch rate 67