Jump to content

Specific Process Knowledge/Thin film deposition/Temescal: Difference between revisions

From LabAdviser
Reet (talk | contribs)
Reet (talk | contribs)
 
(75 intermediate revisions by 4 users not shown)
Line 1: Line 1:
'''Feedback to this page''': '''[mailto:labadviser@danchip.dtu.dk?Subject=Feed%20back%20from%20page%20http://labadviser.danchip.dtu.dk/... click here]'''
'''Feedback to this page''': '''[mailto:labadviser@nanolab.dtu.dk?Subject=Feed%20back%20from%20page%20http://labadviser.nanolab.dtu.dk/index.php?title=Specific_Process_Knowledge/Thin_film_deposition/Temescal click here]'''
<!-- Replace "http://labadviser.danchip.dtu.dk/..." wih the link to the Labadviser page-->
 
 


<i> Unless otherwise stated, this page is written by <b>DTU Nanolab internal</b></i>


==E-Beam Evaporator (Temescal)==
==E-Beam Evaporator (Temescal)==
Line 9: Line 7:
[[File:Temescal.JPG|400px|right|thumb|The Temescal E-beam evaporator in cleanroom A-5]]
[[File:Temescal.JPG|400px|right|thumb|The Temescal E-beam evaporator in cleanroom A-5]]


The Temescal is a system for depositing metals by electron-beam evaporation. In e-beam evaporation, the deposition is line-of-sight directed from the source, which means it will coat only the surface of the sample facing directly towards the source. This makes it very useful for example for metals for lift-off. The system also has an ion source for in-situ Argon sputtering that can be used either for cleaning samples prior to deposition or to modify the film during deposition.  
This system allows electron-beam evaporation of thin films (<1 μm) of metals and one semiconductor, Ge. In e-beam evaporation, the deposition is line-of-sight from the source, which means it will coat only the surface of the sample facing the source directly. This makes it useful for example for [[Specific Process Knowledge/Lithography/LiftOff|lift-off]]. Nanolab's current e-beam evaporators were made by Temescal, a division of FerroTec, and this particular machine was purchased by Nanolab in 2018. It is very similar to the newer e-beam evaporator, bought in 2023, called the [[Specific Process Knowledge/Thin film deposition/10-pocket_e-beam_evaporator|E-beam Evaporator (10-pockets)]] in the LabManager system.
 
A special feature of the 2018 E-beam evaporator (Temescal) is that it has an ion source for argon sputtering. This can be used either for ''in situ'' sample cleaning prior to deposition or to modify the film during deposition (ion beam assisted deposition or IBAD).  


Wafers are loaded into the top of the chamber, which acts as a loadlock as it can be separated from the rest of the chamber by a large gate valve. Deposition will happen on all samples that are loaded together. You can load up to four 6" wafers or three 8" wafers for deposition on surfaces facing the evaporation source, or on up to one 6" wafer for tilted deposition (smaller samples may be tilted more). By using sample holder inserts, you can deposit metals on samples of different sizes and shapes. Only one metal can be deposited at a time, but you can deposit many layers of different metals one after the other. The system contains 6 metals at a time and the metals are exchanged based on user requests, so please request the metals you wish well in advance.  
In both Temescal e-beam evaporators, wafers are loaded into the top of the chamber, which acts as a loadlock as it can be separated from the rest of the chamber by a large gate valve. Deposition will happen on all loaded samples. Up to four 6" wafers /three 8" wafers may be loaded for line-of-sight deposition, or up to one 6" wafer for tilted deposition. Only one material can be deposited at a time, but layers of different metals may be deposited one after the other. The system contains 6 materials at a time which are exchanged weekly based on user requests. Please request materials well in advance.  


'''The user manual, user APV, and contact information can be found in LabManager:'''  
'''The user manual, user APV, and contact information can be found in LabManager:'''  
Line 17: Line 17:


<!-- give the link to the equipment info page in LabManager: -->
<!-- give the link to the equipment info page in LabManager: -->
[http://labmanager.danchip.dtu.dk/function.php?module=Machine&view=view&mach=429 E Beam Evaporator (Temescal) in LabManager]
[http://labmanager.dtu.dk/function.php?module=Machine&view=view&mach=429 E Beam Evaporator (Temescal) in LabManager]
 
'''Training videos may be found here:'''
 
[https://www.youtube.com/playlist?list=PLjWVU97LayHCQWuQyHwddJnpsEYfQp0wf Training videos on Youtube]
 
<br clear="all" />
<br clear="all" />
== Process information ==
== Process information ==


*[[/Acceptance Test|Acceptance Test]]
[[/Acceptance Test|'''Acceptance Test information is found here''']]. Describes '''thickness uniformity''', '''side wall deposition''', '''sheet resistance''', and '''use of the ion source'''.
 
===Materials===
 
[[Specific Process Knowledge/Thin film deposition/Deposition of Aluminium|Aluminium (Al)]]<br>
[[Specific Process Knowledge/Thin film deposition/Deposition of Chromium|Chromium (Cr)]]<br>
[[Specific Process Knowledge/Thin film deposition/Deposition of Copper|Copper (Cu)]]<br>
[[Specific Process Knowledge/Thin film deposition/Deposition of Germanium|Germanium (Ge)]]<br>
[[Specific Process Knowledge/Thin film deposition/Deposition of Gold|Gold (Au)]]<br>
[[Specific Process Knowledge/Thin film deposition/Deposition of Molybdenum|Molybdenum (Mo)]]<br>
[[Specific Process Knowledge/Thin film deposition/Deposition of Nickel|Nickel (Ni)]]<br>
[[Specific Process Knowledge/Thin film deposition/Deposition of Niobium|Niobium (Nb)]]<br>
[[Specific Process Knowledge/Thin film deposition/Deposition of Palladium|Palladium (Pd)]]<br>
[[Specific Process Knowledge/Thin film deposition/Deposition of Platinum|Platinum (Pt)]]<br>
[[Specific Process Knowledge/Thin film deposition/Deposition of Silver|Silver (Ag)]]<br>
[[Specific Process Knowledge/Thin film deposition/Deposition of Tantalum|Tantalum (Ta)]]<br>
[[Specific Process Knowledge/Thin film deposition/Deposition of Tin|Tin (Sn)]] (we recommend using sputtering instead)<br>
[[Specific Process Knowledge/Thin film deposition/Deposition of Titanium|Titanium (Ti)]]<br> 
[[Specific Process Knowledge/Thin film deposition/Deposition of Tungsten|Tungsten (W)]]<br>
 
If your favorite metal is not on the list you are welcome to ask if we can develop a recipe. Note that Si as well as SiO<sub>2</sub>, Al<sub>2</sub>O<sub>3</sub> and other oxides are available on the [[Specific Process Knowledge/Thin film deposition/10-pocket e-beam evaporator|E-beam Evaporator (10-pockets)]].


====Materials for e-beam evaporation====
===Thickness measurement, deposition rate and process control===
How the machine measures the thickness of the growing film using a quartz crystal monitor, how accurately is the control of the rate/thickness, and other useful information about e-beam deposition is found here: [[/Good to know about the Temescal#Deposition rate and thickness measurement accuracy|Thickness, rate, process control]].


*[[Specific Process Knowledge/Thin film deposition/Deposition of Aluminium|Aluminium (Al)]]
===Particulates in the films===
*[[Specific Process Knowledge/Thin film deposition/Deposition of Chromium|Chromium (Cr)]]
Read about optimizing film quality including how to minimize the number of [[/Particulates in Temescal Au films|particulates in Au films in the Temescal]].
*[[Specific Process Knowledge/Thin film deposition/Deposition of Copper|Copper (Cu)]]
*[[Specific Process Knowledge/Thin film deposition/Deposition of Gold|Gold (Au)]]
*[[Specific Process Knowledge/Thin film deposition/Deposition of Molybdenum|Molybdenum (Mo)]]
*[[Specific Process Knowledge/Thin film deposition/Deposition of Nickel|Nickel (Ni)]]
*[[Specific Process Knowledge/Thin film deposition/Deposition of Palladium|Palladium (Pd)]]
*[[Specific Process Knowledge/Thin film deposition/Deposition of Platinum|Platinum (Pt)]]
*[[Specific Process Knowledge/Thin film deposition/Deposition of Silver|Silver (Ag)]]
*[[Specific Process Knowledge/Thin film deposition/Deposition of Tantalum|Tantalum (Ta)]]
*[[Specific Process Knowledge/Thin film deposition/Deposition of Tin|Tin (Sn)]]
*[[Specific Process Knowledge/Thin film deposition/Deposition of Titanium|Titanium (Ti)]] 
*[[Specific Process Knowledge/Thin film deposition/Deposition of Tungsten|Tungsten (W)]] - thinner layers


Note that to date (July 2018) we have processes available for deposition of Al, Cr, Au, Ni, Pd, Ag, Ti, and W as well as Ru. More will be available as they are requested, e.g., Nb is expected in the early fall of 2018.
===Ion source===
[[/Ion source in E-beam evaporator (Temescal)|Information on the ion source]].


==Equipment performance and process related parameters for the Temescal E-beam evaporator==
==Equipment performance and process related parameters==


{| border="2" cellspacing="0" cellpadding="10"  
{| border="2" cellspacing="0" cellpadding="10"  
Line 73: Line 90:
|style="background:LightGrey; color:black"|Process Temperature
|style="background:LightGrey; color:black"|Process Temperature
|style="background:WhiteSmoke; color:black"|
|style="background:WhiteSmoke; color:black"|
*Approximately room temperature
*Approximately room temperature.
Higher for refractive metals that require a lot of heat to evaporate, see above.
|-
|-
|style="background:LightGrey; color:black"|Process pressure
|style="background:LightGrey; color:black"|Process pressure
Line 94: Line 112:
| style="background:LightGrey; color:black"|Substrate material allowed
| style="background:LightGrey; color:black"|Substrate material allowed
|style="background:WhiteSmoke; color:black"|
|style="background:WhiteSmoke; color:black"|
*Silicon wafers
*Almost any that does not outgas and is approved in the cleanroom.
*Quartz wafers
*Pyrex wafers
*See also the [http://labmanager.dtu.dk/function.php?module=XcMachineaction&view=edit&MachID=429 cross-contamination sheet]  
*See also the [http://labmanager.dtu.dk/function.php?module=XcMachineaction&view=edit&MachID=429 cross-contamination sheet]  
|-  
|-  
| style="background:LightGrey; color:black"|Material allowed on the substrate
| style="background:LightGrey; color:black"|Material allowed on the substrate
|style="background:WhiteSmoke; color:black"|
|style="background:WhiteSmoke; color:black"|
*Silicon oxide
*Almost any that does not outgas and is approved in the cleanroom.
*Silicon (oxy)nitride
*Photoresist
*PMMA
*Mylar
*Metals
*See also the [http://labmanager.dtu.dk/function.php?module=XcMachineaction&view=edit&MachID=429 cross-contamination sheet]
*See also the [http://labmanager.dtu.dk/function.php?module=XcMachineaction&view=edit&MachID=429 cross-contamination sheet]
|-  
|-  
|}
|}


'''*''' ''For thicknesses above 600 nm please request permission so we can ensure that enough material will be present.''
'''*''' ''See table in manual with max. allowed rate and cumulative thickness. If you would like to deposit more than the limit in the table, please request permission from metal@nanolab.dtu.dk '''no matter if it is a single layer or a number of deposition runs adding up to a total thickness exceeding the limit'''. This is so we can ensure that enough material will be present and that the the machine can be cleaned up as needed as thick layers can cause flaking.''


'''**''' ''Defined as the ratio of the standard deviation to the average of the measurement made using the DektakXT. For further details see the acceptance test.''
'''**''' ''Defined as the ratio of the standard deviation to the average of the measurement made using the DektakXT. For further details see the acceptance test.''
==Quality control (QC) for the Temescal==
We are still developing the QC procedure for the Temescal (September 2018).
==The e-beam and the Cu hearth==
[[File:Cu hearth.jpg|200px|left|thumb|E-beam impinging on the target from the filament and a 6-pocket Temescal copper hearth and filament assembly enclosed by shields (from Scotech)]]
[[File:Cu hearth 2.jpg|100px|right|thumb|Empty 6-pocket Temescal copper heath (from Fil-Tech)]]
At the start of the deposition and for every 100 nm, please check that the e-beam hits the target material that you would like to evaporate rather than the heath next to the pocket or the bottom of the pocket. I.e., check that the e-beam sweep has not shifted, which could happen if the filament assembly has been distorted by heat for example, and also check that there is enough material in the pocket, so that you do not burn a hole in the bottom of the pocket. If you burn a hole in the bottom of the pocket, cooling water may leak into the chamber and it may flood!
<br clear="all" />
==Thickness measurement==
The machine measures the thickness of the growing film with a Quartz Crystal Microbalance or QCM. The machine calls it the Xtal (crystal). This is a very thin piece of quartz that resonates at about 5-6 MHz when a voltage is applied across it. The resonance frequency varies with the mass of the crystal, and when material is deposited on one side of it, the frequency changes. This is measured by the crystal monitor, which can then calculate the deposited thickness.
[[File:Sell_quartz_crystal_microbalance.jpg|100px|right|thumb|Quartz crystal microbalance with gold electrode. Image from RLC on EC21.com]]
The thickness calculation depends on the material density as well as other physical factors. A so-called ''tooling factor'' is used to adjust the calculation based on the geometry of the setup, since the crystal is not in the same place as the wafer holders and the actual thickness deposited on the crystal is lower than on the samples.
The tooling factor is calibrated for a particular deposition rate. It may not be perfectly accurate for other deposition rates, but should easily be within the 10 % accuracy that we test for in our quality control measurements.
For very thin films the thickness measurement will be less accurate than for thicker films.
The machine gives a rough number for the crystal lifetime simply based on how thick a layer it calculates has been deposited on it. If many layers have been deposited and there is stress in the layers (e.g., in Cr, Ni, or Ru layers), there may be partial delamination, which can make the thickness measurement inaccurate. In this case the lifetime estimate given by the machine will be inaccurate. If you think the crystal is not measuring correctly, please let us know. We exchange the crystals usually around 20 % lifetime use.
<br clear="all" />
== Heating during deposition ==
If the material you are depositing requires a lot of heat to evaporate, the substrates may get warm during the deposition.
A temperature test of a 100 nm Al deposition at 10 Å/s showed that the back of the wafer stays below 37 <sup>o</sup>C. The same is true for 10 nm Ti/90 nm Au at 10 Å/s. In contrast deposition of 60 nm W at about 1 Å/s heated the substrate to above 120 <sup>o</sup>C.
Al requires intermediate power (about 450 mA and 1000 V supplied to the filament that creates the e-beam) while W requires high power (about 600 mA at 1000 V supplied to the filament).
Please ask us if you need to test the heating of the substrates before making a deposition with the metal you need (contact thinfilm@danchip.dtu.dk).

Latest revision as of 21:29, 31 August 2025

Feedback to this page: click here

Unless otherwise stated, this page is written by DTU Nanolab internal

E-Beam Evaporator (Temescal)

The Temescal E-beam evaporator in cleanroom A-5

This system allows electron-beam evaporation of thin films (<1 μm) of metals and one semiconductor, Ge. In e-beam evaporation, the deposition is line-of-sight from the source, which means it will coat only the surface of the sample facing the source directly. This makes it useful for example for lift-off. Nanolab's current e-beam evaporators were made by Temescal, a division of FerroTec, and this particular machine was purchased by Nanolab in 2018. It is very similar to the newer e-beam evaporator, bought in 2023, called the E-beam Evaporator (10-pockets) in the LabManager system.

A special feature of the 2018 E-beam evaporator (Temescal) is that it has an ion source for argon sputtering. This can be used either for in situ sample cleaning prior to deposition or to modify the film during deposition (ion beam assisted deposition or IBAD).

In both Temescal e-beam evaporators, wafers are loaded into the top of the chamber, which acts as a loadlock as it can be separated from the rest of the chamber by a large gate valve. Deposition will happen on all loaded samples. Up to four 6" wafers /three 8" wafers may be loaded for line-of-sight deposition, or up to one 6" wafer for tilted deposition. Only one material can be deposited at a time, but layers of different metals may be deposited one after the other. The system contains 6 materials at a time which are exchanged weekly based on user requests. Please request materials well in advance.

The user manual, user APV, and contact information can be found in LabManager:

E Beam Evaporator (Temescal) in LabManager

Training videos may be found here:

Training videos on Youtube


Process information

Acceptance Test information is found here. Describes thickness uniformity, side wall deposition, sheet resistance, and use of the ion source.

Materials

Aluminium (Al)
Chromium (Cr)
Copper (Cu)
Germanium (Ge)
Gold (Au)
Molybdenum (Mo)
Nickel (Ni)
Niobium (Nb)
Palladium (Pd)
Platinum (Pt)
Silver (Ag)
Tantalum (Ta)
Tin (Sn) (we recommend using sputtering instead)
Titanium (Ti)
Tungsten (W)

If your favorite metal is not on the list you are welcome to ask if we can develop a recipe. Note that Si as well as SiO2, Al2O3 and other oxides are available on the E-beam Evaporator (10-pockets).

Thickness measurement, deposition rate and process control

How the machine measures the thickness of the growing film using a quartz crystal monitor, how accurately is the control of the rate/thickness, and other useful information about e-beam deposition is found here: Thickness, rate, process control.

Particulates in the films

Read about optimizing film quality including how to minimize the number of particulates in Au films in the Temescal.

Ion source

Information on the ion source.

Equipment performance and process related parameters

Purpose Deposition of metals
  • E-beam evaporation of metals
  • Line-of-sight deposition
  • Possible to tilt sample
  • Possible to ion clean samples
  • Possible to modify deposition by Ar ion bombardment
Performance Film thickness
  • 10Å - 1µm* (for some materials)
Deposition rate
  • 0.5Å/s - 10Å/s
Thickness uniformity
  • up to 3 % Wafer-in-Wafer variation, Wafer-to-Wafer and Batch-to-Batch variation **
Thickness accuracy
  • May vary by up to about +/- 10 %
  • Less accurate for films below 20 nm
Process parameter range Process Temperature
  • Approximately room temperature.

Higher for refractive metals that require a lot of heat to evaporate, see above.

Process pressure
  • Below 1*10-6 mbar before deposition starts
  • Below 5*10-6 mbar during deposition
Source-substrate distance
  • 69.85 cm
Substrates Batch size
  • Up to four 6" wafers per standard run
  • Or up to three 8" wafers
  • Up to one 6" wafer with tilt
  • Deposition on one side of the substrate
Substrate material allowed
Material allowed on the substrate

* See table in manual with max. allowed rate and cumulative thickness. If you would like to deposit more than the limit in the table, please request permission from metal@nanolab.dtu.dk no matter if it is a single layer or a number of deposition runs adding up to a total thickness exceeding the limit. This is so we can ensure that enough material will be present and that the the machine can be cleaned up as needed as thick layers can cause flaking.

** Defined as the ratio of the standard deviation to the average of the measurement made using the DektakXT. For further details see the acceptance test.