Jump to content

Specific Process Knowledge/Characterization/XRD: Difference between revisions

From LabAdviser
Khara (talk | contribs)
No edit summary
Reet (talk | contribs)
 
(91 intermediate revisions by 4 users not shown)
Line 1: Line 1:
'''Feedback to this page''': '''[mailto:labadviser@danchip.dtu.dk?Subject=Feed%20back%20from%20page%20http://labadviser.danchip.dtu.dk/... click here]'''
'''Feedback to this page''': '''[mailto:labadviser@nanolab.dtu.dk?Subject=Feed%20back%20from%20page%20http://labadviser.nanolab.dtu.dk/index.php/Specific_Process_Knowledge/Characterization/XRD click here]'''
<!-- Replace "http://labadviser.danchip.dtu.dk/..." wih the link to the Labadviser page-->


== XRD SmartLab ==
<i> Unless otherwise stated, this page is written by <b>DTU Nanolab internal</b></i>


Write a short description of the equipment(s).


[[image:Cluster1.jpg|200x200px|right|thumb|Image(s) of the equipment(s)]]
=XRD at DTU Nanolab=
We have three X-ray diffraction setups in building 346:
*The [[/XRD_SmartLab|XRD SmartLab]] primarily for thin film analysis inside the cleanroom.
*The [[/XRD SmartLab 9kW Rotating Anode|XRD SmartLab 9kW Rotating Anode]] multipurpose system outside the cleanroom.
*The [[/XRD_Powder|XRD Powder]] for phase analysis of powders outside the cleanroom.


==Experiments performed with XRD==
*[[/Process Info|List and description of possible XRD measurements with typical setup requirements]] Note mostly relevant for XRD Smartlab and XRD Rot Anode


'''The user manual(s), quality control procedure(s) and results, user APV(s), technical information and contact information can be found in LabManager:'''
==Data analysis==
<!-- remember to remove the type of documents that are not present -->
For data analysis, we recommend using Rigaku SmartLab Studio for both thinfilms and basic powder analysis.
If more advanced powder analysis is needed we provide access to a remote desktop with a licence for the excellent Malvern Panalytical software, HighScore.


<!-- give the link to the equipment info page in LabManager: -->
*[[/software|Installing SmartLab Studio II]]
[http://labmanager.danchip.dtu.dk/function.php?module=Machine&view=view&mach=326  RIE1 in LabManager]
*[[/dataconversion|Converting data from XRD Powder to SmartLab Studio II]]
*[[/SLSII_analysis|Guide for using SmartLab Studio II for data analysis]]
*[[/HighScore_analysis|Guide for using HighScore Plus for advanced powder data analysis]]
*[[/XRD_Reference_Data|How to download reference spectra for individual crystal structures]] (for DTU users and others with access to the ICSD).


== Process information ==
Apart from commercial software a wide range of free software is available online for data analysis. Please let us know if you find something you'd like to recommend!


Link to process pages - e.g. one page for each material
==Comparison of the XRDs at Nanolab==
 
Example:
*[[Specific Process Knowledge/Etch/Etching of Silicon/Si etch using RIE1 or RIE2|Etch of silicon using RIE]]
*[[Specific Process Knowledge/Etch/Etching of Silicon Oxide/SiO2 etch using RIE1 or RIE2|Etch of silicon oxide using RIE]]
*[[Specific Process Knowledge/Etch/Etching of Silicon Nitride/Etch of Silicon Nitride using RIE|Etch of silicon nitride using RIE]]
*[[Specific Process Knowledge/Etch/Etching of Polymer/Etch of Photo Resist using RIE|Etch of photo resist using RIE]]
 
==Equipment performance and process related parameters==


{| border="2" cellspacing="0" cellpadding="2"  
{| border="2" cellspacing="0" cellpadding="2"  


!colspan="2" border="none" style="background:silver; color:black;" align="center"|Equipment  
!colspan="2" border="none" style="background:silver; color:black;" align="center"|Equipment  
|style="background:WhiteSmoke; color:black"|<b>Equipment 1</b>
|style="background:WhiteSmoke; color:black"|<b>XRD SmartLab</b>
|style="background:WhiteSmoke; color:black"|<b>Equipment 2</b>
|style="background:WhiteSmoke; color:black"|<b>XRD RotAnode</b>
|style="background:WhiteSmoke; color:black"|<b>XRD Powder</b>
|-
|-
!style="background:silver; color:black;" align="center" width="60"|Purpose  
!style="background:silver; color:black;" align="center" width="60"|Purpose  
|style="background:LightGrey; color:black"|  
|style="background:LightGrey; color:black"| Crystal structure analysis
 
and thin film thickness measurement
|style="background:WhiteSmoke; color:black"|
*Phase ID
*Crystal Size
*Crystallinity
*Quality and degree of orientation
*3D orientation
*Lattice strain
*Composition
*Twist
*3D lattice constant
*Thickness
*Roughness
*Density
|style="background:WhiteSmoke; color:black"|
*Phase ID
*Crystal Size
*Crystallinity
*Quality and degree of orientation
*3D orientation
*Lattice strain
*Composition
*Twist
*3D lattice constant
*Thickness
*Roughness
*Density
|style="background:WhiteSmoke; color:black"|
*Phase ID
*Crystal Size
*Crystallinity
|-
!style="background:silver; color:black" align="center" valign="center" rowspan="6"|X-ray generator
|style="background:LightGrey; color:black"|
Maximum rated output
|style="background:WhiteSmoke; color:black"|
3 kW
|style="background:WhiteSmoke; color:black"|
9 kW
|style="background:WhiteSmoke; color:black"|
600 W
|-
|style="background:LightGrey; color:black"|
Rated tube voltage
|style="background:WhiteSmoke; color:black"|
20 to 45 kV
|style="background:WhiteSmoke; color:black"|
20 to 45 kV
|style="background:WhiteSmoke; color:black"|
40 kV
|-
|style="background:LightGrey; color:black"|
Rated tube current
|style="background:WhiteSmoke; color:black"|
2 to 60 mA
|style="background:WhiteSmoke; color:black"|
2 to 200 mA
|style="background:WhiteSmoke; color:black"|
15 mA
|-
|style="background:LightGrey; color:black"|
Type
|style="background:WhiteSmoke; color:black"|
Sealed tube
|style="background:WhiteSmoke; color:black"|
Rotating Anode
|style="background:WhiteSmoke; color:black"|
Sealed tube
|-
|style="background:LightGrey; color:black"|
Target
|style="background:WhiteSmoke; color:black"|
Cu
|style="background:WhiteSmoke; color:black"|
Cu
|style="background:WhiteSmoke; color:black"|
Cu
|-
|style="background:LightGrey; color:black"|
Focus size
|style="background:WhiteSmoke; color:black"|
0.4 mm x 8 mm (Line/Point)
|style="background:WhiteSmoke; color:black"|
|style="background:WhiteSmoke; color:black"|
*Purpose 1
0.1-0.5 mm x 8 mm (Line/Point)
*Purpose 2
|style="background:WhiteSmoke; color:black"|
|style="background:WhiteSmoke; color:black"|
*Purpose 1
0.4 mm x 12 mm (Line)
*Purpose 2
*Purpose 3
|-
|-
!style="background:silver; color:black" align="center" valign="center" rowspan="2"|Performance
!style="background:silver; color:black" align="center" valign="center" rowspan="4"|Goniometer
|style="background:LightGrey; color:black"|Response 1
|style="background:LightGrey; color:black"|
Scanning mode
|style="background:WhiteSmoke; color:black"|
|style="background:WhiteSmoke; color:black"|
*Performance range 1
incident / receiver coupled or independent
*Performance range 2
|style="background:WhiteSmoke; color:black"|
|style="background:WhiteSmoke; color:black"|
*Performance range 1
incident / receiver coupled or independent
*Performance range 2
|style="background:WhiteSmoke; color:black"|
*Performance range 3
incident / receiver coupled
|-
|-
|style="background:LightGrey; color:black"|Response 2
|style="background:LightGrey; color:black"|
Goniomenter radius
|style="background:WhiteSmoke; color:black"|
|style="background:WhiteSmoke; color:black"|
*Performance range
300 mm
|style="background:WhiteSmoke; color:black"|
|style="background:WhiteSmoke; color:black"|
*Performance range
300 mm
|style="background:WhiteSmoke; color:black"|
145 mm
|-
|-
!style="background:silver; color:black" align="center" valign="center" rowspan="2"|Process parameter range
|style="background:LightGrey; color:black"|
|style="background:LightGrey; color:black"|Parameter 1
Minimum step size
|style="background:WhiteSmoke; color:black"|
|style="background:WhiteSmoke; color:black"|
*Range
0.0001° (0.36")
|style="background:WhiteSmoke; color:black"|
|style="background:WhiteSmoke; color:black"|
*Range
0.0001° (0.36")
|style="background:WhiteSmoke; color:black"|
0.001° (3.6")
|-
|-
|style="background:LightGrey; color:black"|Parameter 2
|style="background:LightGrey; color:black"|
Sample stage motion
|style="background:WhiteSmoke; color:black"|
|style="background:WhiteSmoke; color:black"|
*Range
*&chi;:-5~+95°
*&phi;:0~360°
*Z:-4~+1 mm
*X,Y:&plusmn;50 mm for a 100 mm wafer
*Rx,Ry:-5~+5°
|style="background:WhiteSmoke; color:black"|
|style="background:WhiteSmoke; color:black"|
*Range
*&chi;:-5~+95°
*&phi;:0~360°
*Z:-4~+1 mm
*X,Y:&plusmn;50 mm for a 100 mm wafer
*Rx,Ry:-5~+5°
|style="background:WhiteSmoke; color:black"|
Fixed with rotation
 
|-
!style="background:silver; color:black" align="center" valign="center" rowspan="2"|Optics
|style="background:LightGrey; color:black"|Incident side
|style="background:WhiteSmoke; color:black"|
*Cross Beam Optics(CBO)
*Ge(220)x2 monochromator
*In-Plane Parallel Slit Collimator (PSC)
*Soller slit
*Automatic variable divergence slit
*Length limiting slits
|style="background:WhiteSmoke; color:black"|
*Cross Beam Optics(CBO)
*Ge(400)x2 monochromator
*In-Plane Parallel Slit Collimator (PSC)
*Soller slit
*Automatic variable divergence slit
*Length limiting slits
|style="background:WhiteSmoke; color:black"|
*0.04° soller slit
*Ni and Cu filter
*Divergence slits
*Beam masks
|-
|style="background:LightGrey; color:black"|Receiver side
|style="background:WhiteSmoke; color:black"|
*Automatic variable scattering slit
*Automatic variable receiver slit
*Parallel slit analysers (PSA)
*Ge(220)x2 analyser
|style="background:WhiteSmoke; color:black"|
*Automatic variable scattering slit
*Automatic variable receiver slit
*Parallel slit analysers (PSA)
*Ge(400)x2 analyser
|style="background:WhiteSmoke; color:black"|
*0.04° soller slit
*Ni filter
|-
|-
!style="background:silver; color:black" align="center" valign="center" rowspan="3"|Substrates
!style="background:silver; color:black" align="center" valign="center" rowspan="3"|Substrates
|style="background:LightGrey; color:black"|Batch size
|style="background:LightGrey; color:black"|Measurement temperature
|style="background:WhiteSmoke; color:black"|
Room temperature
|style="background:WhiteSmoke; color:black"|
Room temperature
|style="background:WhiteSmoke; color:black"|
May be heated in N<sub><sub>2</sub></sub> up to 500°C
|-
|style="background:LightGrey; color:black"|Substrate size
|style="background:WhiteSmoke; color:black"|
up to 150 mm wafers
 
Thickness max 21 mm
|style="background:WhiteSmoke; color:black"|
|style="background:WhiteSmoke; color:black"|
*<nowiki>#</nowiki> small samples
up to 150 mm wafers
*<nowiki>#</nowiki> 50 mm wafers
 
*<nowiki>#</nowiki> 100 mm wafers
Thickness max 21 mm
*<nowiki>#</nowiki> 150 mm wafers
|style="background:WhiteSmoke; color:black"|
|style="background:WhiteSmoke; color:black"|
*<nowiki>#</nowiki> small samples
Only for powders
*<nowiki>#</nowiki> 50 mm wafers
*<nowiki>#</nowiki> 100 mm wafers
*<nowiki>#</nowiki> 150 mm wafers
|-
|-
| style="background:LightGrey; color:black"|Allowed materials
| style="background:LightGrey; color:black"|Allowed materials
|style="background:WhiteSmoke; color:black"|
|style="background:WhiteSmoke; color:black"|
*Allowed material 1
All materials approved in the cleanroom.
*Allowed material 2
 
No powders or dusty materials.
|style="background:WhiteSmoke; color:black"|
All materials have to be approved
|style="background:WhiteSmoke; color:black"|
|style="background:WhiteSmoke; color:black"|
*Allowed material 1
All materials have to be approved
*Allowed material 2
*Allowed material 3
|-  
|-  
|}
|}


<br clear="all" />
<br clear="all" />

Latest revision as of 23:02, 2 July 2025

Feedback to this page: click here

Unless otherwise stated, this page is written by DTU Nanolab internal


XRD at DTU Nanolab

We have three X-ray diffraction setups in building 346:

Experiments performed with XRD

Data analysis

For data analysis, we recommend using Rigaku SmartLab Studio for both thinfilms and basic powder analysis. If more advanced powder analysis is needed we provide access to a remote desktop with a licence for the excellent Malvern Panalytical software, HighScore.

Apart from commercial software a wide range of free software is available online for data analysis. Please let us know if you find something you'd like to recommend!

Comparison of the XRDs at Nanolab

Equipment XRD SmartLab XRD RotAnode XRD Powder
Purpose Crystal structure analysis

and thin film thickness measurement

  • Phase ID
  • Crystal Size
  • Crystallinity
  • Quality and degree of orientation
  • 3D orientation
  • Lattice strain
  • Composition
  • Twist
  • 3D lattice constant
  • Thickness
  • Roughness
  • Density
  • Phase ID
  • Crystal Size
  • Crystallinity
  • Quality and degree of orientation
  • 3D orientation
  • Lattice strain
  • Composition
  • Twist
  • 3D lattice constant
  • Thickness
  • Roughness
  • Density
  • Phase ID
  • Crystal Size
  • Crystallinity
X-ray generator

Maximum rated output

3 kW

9 kW

600 W

Rated tube voltage

20 to 45 kV

20 to 45 kV

40 kV

Rated tube current

2 to 60 mA

2 to 200 mA

15 mA

Type

Sealed tube

Rotating Anode

Sealed tube

Target

Cu

Cu

Cu

Focus size

0.4 mm x 8 mm (Line/Point)

0.1-0.5 mm x 8 mm (Line/Point)

0.4 mm x 12 mm (Line)

Goniometer

Scanning mode

incident / receiver coupled or independent

incident / receiver coupled or independent

incident / receiver coupled

Goniomenter radius

300 mm

300 mm

145 mm

Minimum step size

0.0001° (0.36")

0.0001° (0.36")

0.001° (3.6")

Sample stage motion

  • χ:-5~+95°
  • φ:0~360°
  • Z:-4~+1 mm
  • X,Y:±50 mm for a 100 mm wafer
  • Rx,Ry:-5~+5°
  • χ:-5~+95°
  • φ:0~360°
  • Z:-4~+1 mm
  • X,Y:±50 mm for a 100 mm wafer
  • Rx,Ry:-5~+5°

Fixed with rotation

Optics Incident side
  • Cross Beam Optics(CBO)
  • Ge(220)x2 monochromator
  • In-Plane Parallel Slit Collimator (PSC)
  • Soller slit
  • Automatic variable divergence slit
  • Length limiting slits
  • Cross Beam Optics(CBO)
  • Ge(400)x2 monochromator
  • In-Plane Parallel Slit Collimator (PSC)
  • Soller slit
  • Automatic variable divergence slit
  • Length limiting slits
  • 0.04° soller slit
  • Ni and Cu filter
  • Divergence slits
  • Beam masks
Receiver side
  • Automatic variable scattering slit
  • Automatic variable receiver slit
  • Parallel slit analysers (PSA)
  • Ge(220)x2 analyser
  • Automatic variable scattering slit
  • Automatic variable receiver slit
  • Parallel slit analysers (PSA)
  • Ge(400)x2 analyser
  • 0.04° soller slit
  • Ni filter
Substrates Measurement temperature

Room temperature

Room temperature

May be heated in N2 up to 500°C

Substrate size

up to 150 mm wafers

Thickness max 21 mm

up to 150 mm wafers

Thickness max 21 mm

Only for powders

Allowed materials

All materials approved in the cleanroom.

No powders or dusty materials.

All materials have to be approved