Specific Process Knowledge/Etch/Wet Titanium Etch: Difference between revisions
Appearance
| (8 intermediate revisions by 2 users not shown) | |||
| Line 1: | Line 1: | ||
'''Feedback to this page''': '''[mailto:wetchemistry@ | '''Feedback to this page''': '''[mailto:wetchemistry@nanolab.dtu.dk?Subject=Feed%20back%20from%20page%20http://labadviser.nanolab.dtu.dk/index.php/Specific_Process_Knowledge/Etch/Wet_Titanium_Etch click here]''' | ||
'''Unless anything else is stated, everything on this page, text and pictures are made by DTU Nanolab.''' | |||
'''All links to Kemibrug (SDS) and Labmanager Including APV requires login.''' | |||
'''All measurements on this page has been made by Nanolab staff.''' | |||
[[Category: Equipment|Etch Wet Titanium]] | [[Category: Equipment|Etch Wet Titanium]] | ||
| Line 7: | Line 13: | ||
==Wet etching of Titanium== | ==Wet etching of Titanium== | ||
[[Image:Fumehood1-2.jpg|300x300px|thumb|Fume hood 01 and 02 in Cleanroom D-3 for working with acids and bases.<br>Wet etching of titanium can be done in beakers with BHF or RCA1 mix in a beaker in one of these fume hoods]] | |||
[[Image:Fumehood1-2.jpg|300x300px|thumb|Fume hood | |||
We have two solutions for wet titanium etching: | We have two solutions for wet titanium etching: | ||
# BHF ( | # BHF (beaker in fumehood) | ||
# Cold RCA1 (fumehood) | # Cold RCA1 (beaker in fumehood) | ||
<br> | |||
Etching titanium in BHF or RCA1 mix is made by making your own solution in a beaker in either Fumehood 01 or 02 in Cleanroom D-3. You can see the APV [http://labmanager.danchip.dtu.dk/d4Show.php?id=2479&mach=146 here]. | |||
| Line 38: | Line 43: | ||
|'''Link to safety APV and KBA''' | |'''Link to safety APV and KBA''' | ||
|[http://labmanager.dtu.dk/d4Show.php?id=4748&mach=368 see APV here] | |[http://labmanager.dtu.dk/d4Show.php?id=4748&mach=368 see APV here] | ||
[ | [https://kemibrug.dk/Kemikalier?stofnavn=BHF See SDS here (requires Kemibrug login)] | ||
|[http://labmanager.dtu.dk/d4Show.php?id=4748&mach=368 see APV here] | |[http://labmanager.dtu.dk/d4Show.php?id=4748&mach=368 see APV here] | ||
|- | |- | ||
| Line 44: | Line 49: | ||
|-style="background:WhiteSmoke; color:black" | |-style="background:WhiteSmoke; color:black" | ||
|'''Chemical solution''' | |'''Chemical solution''' | ||
|HF:NH<sub>4</sub>F | |HF : NH<sub>4</sub>F : NH<sub>4</sub>HF<sub>2</sub> | ||
|H<sub>2</sub>O : NH<sub>4</sub>OH : H<sub>2</sub>O<sub>2</sub> - 5:1:1 | |||
|- | |- | ||
| Line 69: | Line 74: | ||
Not known (it bubbles while etching) | Not known (it bubbles while etching) | ||
| | | | ||
50 nm etches in around 2 min | |||
|- | |- | ||
| Line 75: | Line 80: | ||
!Batch size | !Batch size | ||
| | | | ||
1-5 | 1-5 wafers in beaker | ||
| | | | ||
1-5 | 1-5 wafers in beaker | ||
|- | |- | ||
| Line 90: | Line 94: | ||
!Allowed materials | !Allowed materials | ||
| | | | ||
Practically no restrictions when used in beaker. Make sure to use a plastic beaker, since glass will be attacked by BHF/HF. | |||
Make a note on the beaker of which materials have been processed. | Make a note on the beaker of which materials have been processed. | ||
| | | | ||
Practically no restrictions when used in beaker. | |||
Make a note on the beaker of which materials have been processed. | Make a note on the beaker of which materials have been processed. | ||
|- | |- | ||
|} | |} | ||