== The nano1.21 recipe ==
== The nano1.21 recipe ==
<!-- revised 1/6-2015 by jmli -->


{| border="2" cellpadding="2" cellspacing="1"  
{| border="2" cellpadding="2" cellspacing="1"  
Line 75: Line 82:




<-- revised -->
<!-- revised -->

Latest revision as of 08:41, 4 April 2025



The nano1.21 recipe

Recipe nano1.21
Recipe Gas C4F8 75 sccm, SF6 38 sccm
Pressure 4 mTorr, Strike 3 secs @ 15 mTorr
Power 800 W CP, 50 W PP
Temperature -10 degs
Hardware 100 mm Spacers
Time 120 secs
Conditions Run ID 1925
Conditioning Sequence: Oxygen clean, MU tests, processes, no oxygen between runs
Mask 211 nm zep etched down to 74 nm



Nominal trench line width ' 30 60 90 120 150 Avg Std
Etch rates nm/min 168 182 185 189 191 183 9
Sidewall angle degs 91 91 91 91 90 91 0
CD loss nm/edge 7 -3 -3 -25 -26 -10 15
CD loss foot nm/edge 12 9 10 -11 1 4 9
Bowing 9 6 4 5 7 6 2
Bottom curvature -47 -34 -34 -26 -19 -32 10
zep nm/min 69