Jump to content

Specific Process Knowledge/Thin film deposition/Deposition of Silicon Oxide/Deposition of Silicon Oxide using PECVD: Difference between revisions

Bghe (talk | contribs)
Bghe (talk | contribs)
 
(76 intermediate revisions by 2 users not shown)
Line 1: Line 1:
'''Feedback to this page''': '''[mailto:labadviser@danchip.dtu.dk?Subject=Feed%20back%20from%20page%20http://labadviser.danchip.dtu.dk/index.php/Specific_Process_Knowledge/Thin_film_deposition/Deposition_of_Silicon_Oxide/Deposition_of_Silicon_Oxide_using_PECVD  click here]'''  
'''Feedback to this page''': '''[mailto:labadviser@nanolab.dtu.dk?Subject=Feed%20back%20from%20page%20http://labadviser.nanolab.dtu.dk/index.php/Specific_Process_Knowledge/Thin_film_deposition/Deposition_of_Silicon_Oxide/Deposition_of_Silicon_Oxide_using_PECVD  click here]'''<br>
{{CC-bghe1}}




At the moment DANCHIP has 2(3) PECVDs that can deposite silicon oxide with or without dopants of Boron, Phosphorous or Germanium. PECVD1 has been decommissioned and PECVD3 are for silicon based processing allowing wafers with small abount of metal (<5% wafer coverage). PECVD2 is for clean wafers both for silicon based materials and for III-V materials. Look at the [[Specific Process Knowledge/Thin film deposition/PECVD|PECVD]] page to learn more about the PECVDs at DANCHIP. All though PECVD2 and PECVD3 are very much alike you cannot count on that a recipe on one system will give exactly the same results on the other system.
At the moment DTU Nanolab has 2 PECVDs that can deposit silicon oxide with or without dopants of boron, phosphorus. PECVD1 and PECVD2 has been decommissioned and now we have PECVD3 and PECVD4. PECVD3 are for silicon based processing allowing wafers with small amount of metal (<5% wafer coverage). PECVD4 is for clean wafers both for silicon based materials and for III-V materials. Look at the [[Specific Process Knowledge/Thin film deposition/PECVD|PECVD]] page to learn more about the PECVDs at Nanolab. All though PECVD4 and PECVD3 are very much alike you cannot count on that a recipe on one system will give exactly the same results on the other system.


=Recipes on PECVD2 for deposition of silicon oxides=
== Deposition of SiO2 with PECVD4 ==
{| border="1" cellspacing="2" cellpadding="2" colspan="3"
|bgcolor="#98FB98" |'''Quality Control (QC) for PECVD4 - oxide '''
|-
|
*[http://labmanager.dtu.dk/d4Show.php?id=5093&mach=395 The QC procedure for PECVD4 - requires login]<br>
*[https://labmanager.dtu.dk/view_binary.php?type=data&mach=395 The newest QC data for PECVD4 - requires login]
{| {{table}}
| align="center" |
{| border="1" cellspacing="1" cellpadding="2"  align="center" style="width:200px"
 
! QC Recipe:
! QCOXYD2
|-
| SiH<sub>4</sub> flow
|12 sccm
|-
|N<sub>2</sub>O flow
|1420 sccm
|-
|N<sub>2</sub> flow
|392 sccm
 
|-
|Pressure
|550 mTorr
|-
|RF-power
|60 W
|-
|}
| align="center" valign="top"|
{| border="2" cellspacing="1" cellpadding="2" align="center" style="width:500px"
!QC limits
!PECVD4 - OXIDE
|-
|Deposition rate
|70 - 85 nm/min
|-
|Non-uniformity
|<3.0
|-
|Refractive index
|1.474 - 1.486
|-
|}
|-
|}
|}
 
{| border="1" cellspacing="2" cellpadding="2"
|-style="background:Black; color:White"
!|Recipe
!|Dep. rate [nm/min]
!|RI
!|Unif. [%]
!|Stress [MPa]
!|Comments
!|SiH4 [sccm]
!|N2O [sccm]
!|N2 [sccm]
!|B2H6
!|PH3
!|Pressure [mTorr]
!|Power [W]
!|Load
!|Tune
!|Time [mm:ss]
!|Tested
|-
|LF SiO<!-- Recipe -->
|75-78 nm/min<!-- Dep. rate [nm/min] -->
|1.480-1.483<!-- RI -->
|&plusmn; 2.1-2.7%<!-- Unif. [%] -->
|compressive 309 MPa <!-- Stress [MPa] -->
|[[/LF_SiO2 results|Click for more results]]<!-- Comments -->
|12<!-- SiH4 [sccm] -->
|1420<!-- N2O [sccm] -->
|392<!-- N2 [sccm] -->
|<!-- B2H6 -->
|<!-- PH3 -->
|550 mTorr<!-- Pressure [mTorr] -->
|60LF"<!-- Power [W] -->
|<!-- Load -->
|<!-- Tune -->
|1:15/13:00(stress)<!-- Time [mm:ss] -->
|February 2017 bghe<!--Tested -->
|-
|HF SiO<!-- Recipe -->
|63-64 nm/min<!-- Dep. rate [nm/min] -->
|1.476-1.477<!-- RI -->
|&plusmn; 0.3-0.5%<!-- Unif. [%] -->
|Compressive: 250.5 MPa<!-- Stress [MPa] -->
|[[/HF_SiO2 results|Click for more results]]<!-- Comments -->
|10<!-- SiH4 [sccm] -->
|1420<!-- N2O [sccm] -->
|392<!-- N2 [sccm] -->
|<!-- B2H6 -->
|<!-- PH3 -->
|900 mTorr<!-- Pressure [mTorr] -->
|30HF<!-- Power [W] -->
|<!-- Load -->
|<!-- Tune -->
|2:00/16:00(stress)<!-- Time [mm:ss] -->
|February 2017 bghe<!--Tested -->
|-
|waveguide <!-- Recipe -->
|159.5 nm/min<!-- Dep. rate [nm/min] -->
|1.462<!-- RI -->
|&plusmn; 0.8%<!-- Unif. [%] -->
|Compressive: 121.9 MPa<!-- Stress [MPa] -->
|<!-- Comments -->
|17<!-- SiH4 [sccm] -->
|2000<!-- N2O [sccm] -->
|<!-- N2 [sccm] -->
|<!-- B2H6 -->
|<!-- PH3 -->
|300 mTorr<!-- Pressure [mTorr] -->
|700 LF<!-- Power [W] -->
|<!-- Load -->
|<!-- Tune -->
|40:00<!-- Time [mm:ss] -->
|February 2017 bghe<!--Tested -->
|-
|BPSG<!-- Recipe -->
|259 nm/min<!-- Dep. rate [nm/min] -->
|1.4593<!-- RI -->
|&plusmn; 1.7%<!-- Unif. [%] -->
|Compressive: 36.7 MPa<!-- Stress [MPa] -->
|Measured after anneal in Clad1000<!-- Comments -->
|17<!-- SiH4 [sccm] -->
|1600<!-- N2O [sccm] -->
|<!-- N2 [sccm] -->
|135<!-- B2H6 -->
|40<!-- PH3 -->
|900 mTorr<!-- Pressure [mTorr] -->
|800 LF <!-- Power [W] -->
|<!-- Load -->
|<!-- Tune -->
|10:00/56:00(stress)<!-- Time [mm:ss] -->
|February 2017 bghe <!--Tested -->
|-
|BPSG low stress<!-- Recipe -->
|302 nm/min<!-- Dep. rate [nm/min] -->
|1.4598<!-- RI -->
|&plusmn; 1.7%<!-- Unif. [%] -->
|Compressive: 1.4 MPa<!-- Stress [MPa] -->
|Measured after anneal in Clad1000 <!-- Comments -->
|17<!-- SiH4 [sccm] -->
|1600<!-- N2O [sccm] -->
|<!-- N2 [sccm] -->
|240<!-- B2H6 -->
|60<!-- PH3 -->
|500 mTorr<!-- Pressure [mTorr] -->
|800LF<!-- Power [W] -->
|<!-- Load -->
|<!-- Tune -->
|10:00 <!-- Time [mm:ss] -->
|February 2017 bghe <!--Tested -->
 
|-
 
|}
 
*[[/conformity|SEM images of the conformity of the layer on a structured surface]]
 
<br clear="all" />
 
=Recipes on PECVD3 for deposition of silicon oxides=
{| border="1" cellspacing="2" cellpadding="2" colspan="3"
|bgcolor="#98FB98" |'''Quality Control (QC) for PECVD3 - oxide'''
|-
|
*[http://labmanager.dtu.dk/d4Show.php?id=1402&mach=106 The QC procedure for PECVD3 - requires login]<br>
*[https://labmanager.dtu.dk/view_binary.php?type=data&mach=106 The newest QC data for PECVD3 - requires login]
{| {{table}}
| align="center" |
{| border="1" cellspacing="1" cellpadding="2"  align="center" style="width:200px"
 
! QC Recipe:
! QCOXYD2
|-
| SiH<sub>4</sub> flow
|12 sccm
|-
|N<sub>2</sub>O flow
|1420 sccm
|-
|N<sub>2</sub> flow
|392 sccm
 
|-
|Pressure
|700 mTorr
|-
|RF-power
|150 W
|-
|}
| align="center" valign="top"|
{| border="2" cellspacing="1" cellpadding="2" align="center" style="width:500px"
!QC limits
!PECVD3 - OXIDE
|-
|Deposition rate
|97 - 112 nm/min
|-
|Non-uniformity
|<2.0
|-
|Refractive index
|1.467 - 1.474
|-
|}
|-
|}
|}
 
===Recipes===
{| border="1" cellspacing="0" cellpadding="7"
|-
|Recipe name
|SiH4 flow [sccm]
|N<sub>2</sub>O flow [sccm]
|N2 flow [sccm]
|B2H6 flow [sccm]
|PH3 flow [sccm]
|Pressure [mTorr]
|Power [W]
|Description
|-
|LFSiO2
|12
|1420
|392
|0
|0
|700
|150
|New QC implemented in April 2016
|-
|LFSiO
|12
|1420
|392
|0
|0
|550
|60
|Uniform silicon oxide
|-
|1PBSG
|17
|1600
|0
|135
|40
|500
|800 LF
|BPSG glass for waveguide cladding layer
|}
LF=Low Frequency
 
===Expected results===
{| border="1" cellspacing="0" cellpadding="5"
|-
|Recipe name
|Deposition rate [nm/min]
|RI
|Uniformity [%]
|Stress
|Comment
|-
|LFSiO2
|105nm/min
|1.47
|~1.5%
|'''400-402 MPa''' compressive stress '' by Anders Simonsen @nbi.ku.dk April 2016''
|We have seen that this recipe does not deposit the first minute
|-
|LFSiO
|~75
|~1.48
|<1
|not measured
|.
|-
|1PBSG
|~228 nm/min
|.
|~17%
|not measured
|.
|}
<br clear="all" />
 
=Recipes on PECVD3 for deposition of doped oxide=
===Recipes===
{| border="1" cellspacing="0" cellpadding="7"
|-
|Recipe name
|SiH<sub>4</sub> flow [sccm]
|N<sub>2</sub>O flow [sccm]
|N<sub>2</sub> flow [sccm]
|GeH<sub>4</sub> flow [sccm] (scaled by 100)
|B<sub>2</sub>H<sub>6</sub> flow [sccm]
|PH<sub>3</sub> flow [sccm]
|Pressure [mTorr]
|Power [W]
|Description
|-
|Core-Ge (not possible anymore as we have no Germanium)
|17
|1600
|300
|300
|0
|0
|400
|600 LF
|Process for germanium doped core layer developed by Haiyan Ou from DTU Photonics
Annnealing: Anneal bond furnace, recipe "core1100"
|-
|Top-BPSG
|17
|1600
|0
|0
|100
|40
|500
|800 LF
|Process for PBSG top clading layer developed by Haiyan Ou from DTU Photonics
Annnealing/oxidation: Anneal bond furnace, recipe "clad1000"
|}
 
===Expected results===
{| border="1" cellspacing="0" cellpadding="5"
|-
|Recipe name
|Deposition rate [nm/min]
|Refractive index
|-
|Core-Ge
|~188 nm/min
|~1.46969
|-
|Top-BPSG
|~248 nm/min
|~1.458
|}
 
=Recipes on PECVD2 for deposition of silicon oxides <span style="color:Red">EXPIRED!!!</span>=
   
   
==Quality control recipe==
==Quality control recipe (recipe changed in June 2015)==
{| border="1" cellspacing="2" cellpadding="2" colspan="3"
{| border="1" cellspacing="2" cellpadding="2" colspan="3"
|bgcolor="#98FB98" |'''Quality Controle (QC) for PECVD2'''
|bgcolor="#98FB98" |'''Quality Controle (QC) for PECVD2'''
|-
|-
|
|
*[http://labmanager.danchip.dtu.dk/d4Show.php?id=1988&mach=17 The QC procedure for PECVD2]<br>
 
*[http://labmanager.danchip.dtu.dk/function.php?module=Machine&view=view&mach=17 The newest QC data for PECVD2]
{| {{table}}
{| {{table}}
| align="center" |  
| align="center" |  
Line 30: Line 384:
|-  
|-  
|Pressure
|Pressure
|550 mTorr
|700 mTorr
|-
|-
|RF-power
|RF-power
|100 W @380kHz
|150 W @380kHz
|-
|-
|Deposition time
|Deposition time
|1 min
|15 min
|}
|}
| align="center" valign="top"|
| align="center" valign="top"|
Line 43: Line 397:
!PECVD2
!PECVD2
|-
|-
|Depostion rate of Silicon Oxide
|Deposition rate of Silicon Oxide
|69nm/min - 119nm/min
|58 nm/min - 78nm/min
|-
|-
|Non-uniformity of the deposition rate (std. deviation of 9 points)
|Non-uniformity of the deposition rate: ''(max-min)/2*AVG''
|0 - 2.8 nm
|<2%
|-
|-
|Refractive index of the Silicon Oxide
|Refractive index of the Silicon Oxide
|1.41 - 1.53
|1.45 - 1.48
|-
|-
|Non-uniformity of the refrative index (std. deviation of 9 points)
|Non-uniformity of the refractive index: ''(max-min)/2*AVG''
|0 - 0.07
|<0.2%
|-
|-
|}
|}
Line 60: Line 414:
|}
|}


==SiO2 Standard, High Rate==
==SiO2, High Rate <span style="color:Red">EXPIRED!!!</span>==






{| border="1" style="text-align: center; width: 400px; height: 150px;"
{| border="1" style="text-align: center; width: 400px; height: 150px;"
! colspan="2" style="text-align: center;" style="background: #efefef;" | SiO2 Standard
! colspan="2" style="text-align: center;" style="background: #efefef;" | 1SiO2HR
|-
|-
!N<math>_2</math>O-flow
!N<math>_2</math>O-flow
Line 80: Line 434:
|-
|-
!Deposition rate
!Deposition rate
|179 nm/min
|179 nm/min (before 2014)
|-
|-
!index of refraction
!index of refraction
|1.461
|1.461 (before 2014)
|}
|}


==SiO2 Standard, Low Rate==
==SiO2 Low Rate <span style="color:Red">EXPIRED!!!</span>==




{| border="1" style="text-align: center; width: 700px; height: 150px;"
{| border="1" style="text-align: center; width: 700px; height: 150px;"
! colspan="2" style="text-align: left;" style="background: #efefef;" | 1STOxide
! colspan="2" style="text-align: left;" style="background: #efefef;" | 1OX_old
! colspan="2" style="text-align: left;" style="background: #efefef;" | A test recipe
! colspan="2" style="text-align: left;" style="background: #efefef;" | 1SiO2 (as QC)
|-
|-
!N<math>_2</math>-flow
!N<math>_2</math>-flow
Line 115: Line 469:
!Deposition rate
!Deposition rate
|~100 nm/min
|~100 nm/min
|109 &plusmn; 2 nm/min [tested: 2014-03-18]
|
'''66 nm/min''' (2015-05-18 BGHE)<br>
'''68-69 nm/min''' (2015-04-24 BGHE)<br>
109 &plusmn; 2 nm/min [tested: 2014-03-18] ''Old shower head''
|-
|-
!index of refraction
!index of refraction
|1.47
|1.47
|1.465 [tested: 2014-03-18]
|
'''1.463-1.464''' (2015-04-24 BGHE)<br>
1.465 [tested: 2014-03-18] ''Old shower head''
|-
|-
!Uniformity
!Uniformity
|<1 %
|<1 %
|3.2% over the wafer [tested: 2014-03-18]
|
'''1%''' over the wafer (2015-04-24 BGHE)<br>
3.2% over the wafer [tested: 2014-03-18] ''Old shower head''
|-
!Comment
|This recipe is not running stable. The load capacitor tunes to zero and that it cannot go further. The results in a small reflected power that is varying due to the bad matching. This lead to variations in results from time to time. You may use it if you like, but please expect some variation in deposition rate.
|This recipe was developed because the old one didn't tune well. It may have a less good uniformity but should be more stable.
|}
|}




===Deposition rate as a function of deposition time using 1STOxide:===
===Deposition rate as a function of deposition time using 1Ox_old:===
{| border="1" style="text-align: center; width: 400px; height: 150px;"
{| border="1" style="text-align: center; width: 400px; height: 150px;"
|-
|-
Line 161: Line 526:
|99.6
|99.6
|}
|}


===Thickness uniformity of test wafer using the test recipe===
===Thickness uniformity of test wafer using the test recipe===
Line 168: Line 532:
<br clear="all" />
<br clear="all" />


==BPSG: RI vs. B/P ==
==BPSG: RI vs. B/P <span style="color:Red">EXPIRED!!!</span> ==
B2H6 flow and PH3 flow was varied to map the RI of different B2H6/PH3 ratios. <br>
B2H6 flow and PH3 flow was varied to map the RI of different B2H6/PH3 ratios. <br>
''Work done by BGHE@danchip in fall 2013'' <br>
''Work done by BGHE@dtu in fall 2013'' <br>
{| border="1" cellspacing="0" cellpadding="7"
{| border="1" cellspacing="0" cellpadding="7"
|-
|-
Line 244: Line 608:
<br clear="all" />
<br clear="all" />


=Recipes on PECVD3 for deposition of silicon oxides=
=Recipes on PECVD1 for deposition of silicon oxides <span style="color:Red">EXPIRED!!!</span>=
{| border="1" cellspacing="2" cellpadding="2" colspan="3"
|bgcolor="#98FB98" |'''Quality Controle (QC) for PECVD3 - oxide'''
|-
|
*[http://labmanager.danchip.dtu.dk/d4Show.php?id=1402&mach=106 The QC procedure for PECVD3]<br>
*[http://www.labmanager.danchip.dtu.dk/view_binary.php?type=data&mach=106 The newest QC data for PECVD3]
{| {{table}}
| align="center" |
{| border="1" cellspacing="1" cellpadding="2"  align="center" style="width:200px"
 
! QC Recipe:
! QCOXYD
|-
| SiH<sub>4</sub> flow
|12 sccm
|-
|N<sub>2</sub>O flow
|1420 sccm
|-
|N<sub>2</sub> flow
|392 sccm
 
|-
|Pressure
|550 mTorr
|-
|RF-power
|60 W
|-
|}
| align="center" valign="top"|
{| border="2" cellspacing="1" cellpadding="2" align="center" style="width:500px"
!QC limits
!PECVD3 - OXIDE
|-
|Deposition rate
|66 - 89 nm/min
|-
|Non-uniformity
|<1.9%
|-
|Refractive index
|1.472 - 1.487
|-
|}
|-
|}
|}
 
===Recipes===
{| border="1" cellspacing="0" cellpadding="7"
|-
|Recipe name
|SiH4 flow [sccm]
|N<sub>2</sub>O flow [sccm]
|N2 flow [sccm]
|B2H6 flow [sccm]
|PH3 flow [sccm]
|Pressure [mTorr]
|Power [W]
|Description
|-
|LFSiO
|12
|1420
|392
|0
|0
|550
|60
|Uniform silicon oxide
|-
|1PBSG
|17
|1600
|0
|135
|40
|500
|800LF
|BPSG glass for waveguide cladding layer
|}
LF=Low Frequency
 
===Expected results===
{| border="1" cellspacing="0" cellpadding="5"
|-
|Recipe name
|Deposition rate [nm/min]
|RI
|Uniformity [%]
|-
|LFSiO
|~75
|~1.48
|<1
|-
|1PBSG
|~228 nm/min
|.
|~17%
|}
<br clear="all" />
 
=Recipes on PECVD3 for deposition of doped oxide=
===Recipes===
{| border="1" cellspacing="0" cellpadding="7"
|-
|Recipe name
|SiH<sub>4</sub> flow [sccm]
|N<sub>2</sub>O flow [sccm]
|N<sub>2</sub> flow [sccm]
|GeH<sub>4</sub> flow [sccm] (scaled by 100)
|B<sub>2</sub>H<sub>6</sub> flow [sccm]
|PH<sub>3</sub> flow [sccm]
|Pressure [mTorr]
|Power [W]
|Description
|-
|Core-Ge
|17
|1600
|300
|300
|0
|0
|400
|600 LF
|Process for germanium doped core layer developed by Haiyan Ou from DTU Photonics
Annnealing: Anneal bond furnace, recipe "core1100"
|-
|Top-BPSG
|17
|1600
|0
|0
|100
|40
|500
|800 LF
|Process for PBSG top clading layer developed by Haiyan Ou from DTU Photonics
Annnealing/oxidation: Anneal bond furnace, recipe "clad1000"
|}
 
===Expected results===
{| border="1" cellspacing="0" cellpadding="5"
|-
|Recipe name
|Deposition rate [nm/min]
|Refractive index
|-
|Core-Ge
|~188 nm/min
|~1.46969
|-
|Top-BPSG
|~248 nm/min
|~1.458
|}
 
 
=Recipes on PECVD1 for deposition of silicon oxides <span style="color:Red">Expired!</span>=
===Recipes===
===Recipes===
{| border="1" cellspacing="0" cellpadding="7"
{| border="1" cellspacing="0" cellpadding="7"