'''Unless anything else is stated, everything on this page, text and pictures are made by DTU Nanolab.'''
'''All links to Kemibrug (SDS) and Labmanager Including APV and QC requires login.'''
'''Feedback to this page''': '''[mailto:labadviser@danchip.dtu.dk?Subject=Feed%20back%20from%20page%20https://labadviser.nanolab.dtu.dk/index.php/Specific_Process_Knowledge/Etch/Etching_of_Aluminium click here]'''
<!--Page reviewed by jmli 1/8-2016  -->
<!-- Ok, jmli 2020-0120 -->
==Etching of Aluminium==
==Etching of Aluminium==
Etching of aluminium is done wet at Danchip. We have two different solutions:


# H<math>_2</math>O:H<math>_3</math>PO<math>_4</math> 1:2 at 50 <sup>o</sup>C
Etching of aluminium can be done either by wet etch, dry etch or by sputtering with ions.
# Pre-mixed etch solution: PES 77-19-04 at 20 <sup>o</sup>C
*[[Specific Process Knowledge/Etch/Wet Aluminium Etch|Etching of Al by wet etch]]
*[[Specific_Process_Knowledge/Etch/ICP_Metal_Etcher/Aluminium|Etching of Al by dry etch]]
*[[Specific_Process_Knowledge/Etch/IBE&frasl;IBSD Ionfab 300|Sputtering of Al]]
<br clear="all" />
 
==Comparison of Aluminium Etch Methods==
 
{|border="1" cellspacing="1" cellpadding="3" style="text-align:left;"
|-
 
|-
|-style="background:silver; color:black"
!
![[Specific Process Knowledge/Etch/Wet Aluminium Etch|Aluminium Etch]]
![[Specific_Process_Knowledge/Lithography/Development#Developer:_TMAH_Manual|Developer TMAH manual]]
![[Specific_Process_Knowledge/Etch/ICP_Metal_Etcher|ICP metal]]
![[Specific_Process_Knowledge/Etch/IBE&frasl;IBSD Ionfab 300|IBE (Ionfab300+)]]
|-
 
|-
|-style="background:WhiteSmoke; color:black"
!Generel description
|Wet etch of Al
|Wet etch/removal: TMAH<br>
Mainly used for removing Al on e-beam resist after e-beam exposure, see process flow [[Specific_Process_Knowledge/Lithography/EBeamLithography#Aluminum_coating| here]]
|Dry plasma etch of Al
|Sputtering of Al - pure physical etch.
|-


{| border="1" cellspacing="0" cellpadding="4" align="center"
|-
!
|-style="background:LightGrey; color:black"
! Aluminium Etch 1
!Etch rate range
! Aluminium Etch 2
|-
|General description
|
|
*Etch of pure aluminium
*~60-100nm/min
|
|
*Etch of aluminium + 1.5% Si
*~30nm/min (pure Al)
|
*~350 nm/min (depending on features size and etch load)
|
*~30nm/min (not tested yet)
|-
 
|-
|-
|Chemical solution
|-style="background:WhiteSmoke; color:black"
!Etch profile
|
|
*Isotropic
|
|
|-
*Isotropic
|Possible masking materials:
|
|
*Photoresist (1.5 µm AZ5214E)
*Anisotropic (vertical sidewalls)
|
|
*Photoresist (1.5 µm AZ5214E)
*Anisotropic (angles sidewalls, typical around 70 dg)
|-
|-
|Etch rate
 
 
|-
|-style="background:LightGrey; color:black"
!Substrate size
|
|
~100 nm/min (Pure Al)
*100 mm wafers (in bath)
*150 mm wafers (in bath)
*Any size (in beaker)
|
|
~60(??) nm/min
*Chips (6-60 mm)  
|-
*100 mm wafers
|Batch size
*150 mm wafers
|
|
*1-25 wafers at a time
*smaller pieces on a carrier wafer
*<nowiki>#</nowiki>1 100mm wafers (when set up to 100mm wafers)
*<nowiki>#</nowiki>1 150mm wafers (when set up to 150mm wafers)
|
|
*1-25 wafer at a time
Smaller pieces glued to carrier wafer
*<nowiki>#</nowiki>1 50mm wafer
*<nowiki>#</nowiki>1 100mm wafer
*<nowiki>#</nowiki>1 150mm wafer
*<nowiki>#</nowiki>1 200mm wafer
|-
 
|-
|-
|Size of substrate
|-style="background:WhiteSmoke; color:black"
!'''Allowed materials'''
|In 'Aluminium Etch' bath:
*See Cross Contamination Sheet for [https://labmanager.dtu.dk/function.php?module=XcMachineaction&view=edit&MachID=381 Aluminium Etch] bath (require login)
In beaker:
*Any material
|
|
*4" wafers
*Every thing that is allowed in the Developer: TMAH Manual
|
*4" wafers
|-
|Allowed materials
|
|
*Silicon
*Quartz/fused silica
*Photoresist/e-beam resist
*PolySilicon,
*Silicon oxide
*Silicon (oxy)nitride
*Aluminium
*Aluminium
*Silicon
*Titanium
*Silicon Oxide
*Chromium
*Silicon Nitride
*Silicon Oxynitride
*Photoresist
*E-beam resist
|
|
*Aluminium
*Silicon
*Silicon
*Silicon oxides
*Silicon Oxide
*Silicon nitrides
*Silicon Nitride
*Metals from the +list
*Silicon Oxynitride
*Metals from the -list
*Photoresist
*Alloys from the above list
*E-beam resist
*Stainless steel
*Glass
*III-V materials
*Resists
*Polymers
*Capton tape
|-
|-
|}
|}

Latest revision as of 13:00, 31 July 2026

Unless anything else is stated, everything on this page, text and pictures are made by DTU Nanolab.

All links to Kemibrug (SDS) and Labmanager Including APV and QC requires login.

Feedback to this page: click here

Etching of Aluminium

Etching of aluminium can be done either by wet etch, dry etch or by sputtering with ions.


Comparison of Aluminium Etch Methods

Aluminium Etch Developer TMAH manual ICP metal IBE (Ionfab300+)
Generel description Wet etch of Al Wet etch/removal: TMAH

Mainly used for removing Al on e-beam resist after e-beam exposure, see process flow here

Dry plasma etch of Al Sputtering of Al - pure physical etch.
Etch rate range
  • ~60-100nm/min
  • ~30nm/min (pure Al)
  • ~350 nm/min (depending on features size and etch load)
  • ~30nm/min (not tested yet)
Etch profile
  • Isotropic
  • Isotropic
  • Anisotropic (vertical sidewalls)
  • Anisotropic (angles sidewalls, typical around 70 dg)
Substrate size
  • 100 mm wafers (in bath)
  • 150 mm wafers (in bath)
  • Any size (in beaker)
  • Chips (6-60 mm)
  • 100 mm wafers
  • 150 mm wafers
  • smaller pieces on a carrier wafer
  • #1 100mm wafers (when set up to 100mm wafers)
  • #1 150mm wafers (when set up to 150mm wafers)

Smaller pieces glued to carrier wafer

  • #1 50mm wafer
  • #1 100mm wafer
  • #1 150mm wafer
  • #1 200mm wafer
Allowed materials In 'Aluminium Etch' bath:

In beaker:

  • Any material
  • Every thing that is allowed in the Developer: TMAH Manual
  • Silicon
  • Quartz/fused silica
  • Photoresist/e-beam resist
  • PolySilicon,
  • Silicon oxide
  • Silicon (oxy)nitride
  • Aluminium
  • Titanium
  • Chromium
  • Silicon
  • Silicon oxides
  • Silicon nitrides
  • Metals from the +list
  • Metals from the -list
  • Alloys from the above list
  • Stainless steel
  • Glass
  • III-V materials
  • Resists
  • Polymers
  • Capton tape