Jump to content

Specific Process Knowledge/Etch/KOH Etch: Difference between revisions

From LabAdviser
Kabi (talk | contribs)
Taran (talk | contribs)
No edit summary
 
(114 intermediate revisions by 7 users not shown)
Line 1: Line 1:
'''Feedback to this page''': '''[mailto:wetchemistry@danchip.dtu.dk?Subject=Feed%20back%20from%20page%20http://labadviser.danchip.dtu.dk/index.php/Specific_Process_Knowledge/Etch/KOH_Etch click here]'''
'''Feedback to this page''': '''[mailto:labadviser@nanolab.dtu.dk?Subject=Feed%20back%20from%20page%20http://labadviser.nanolab.dtu.dk/index.php/Specific_Process_Knowledge/Etch/KOH_Etch click here]'''


'''Unless anything else is stated, everything on this page, text and pictures are made by DTU Nanolab.'''


==KOH etch - ''Anisotropic silicon etch''==
'''All links to Kemibrug (SDS) and Labmanager Including APV and QC requires login.'''
 
 
[[Category:Equipment|Etch Wet KOH etch]]
[[Category:Etch (Wet) bath|KOH etch]]
 
==Si etch - ''Anisotropic silicon etch''==


KOH belongs to the family of anisotropic Si-etchants based on aqueous alkaline solutions. The anisotropy stems from the different etch rates in different crystal directions. The {111}-planes are almost inert whereas the etch rates of e.g. {100}- and {110}-planes are several orders of magnitude faster.
KOH belongs to the family of anisotropic Si-etchants based on aqueous alkaline solutions. The anisotropy stems from the different etch rates in different crystal directions. The {111}-planes are almost inert whereas the etch rates of e.g. {100}- and {110}-planes are several orders of magnitude faster.


KOH-etching is a highly versatile and cheap way to realize micro mechanical structures if you can live with the necessary Si<sub>3</sub>N<sub>4</sub>- or SiO<sub>2</sub>-masking materials and the potassium contamination of the surface. '''The latter necessitates in most cases a wet post-clean ([[Specific Process Knowledge/Wafer cleaning/7-up & Piranha|'7-up']] or [[Specific Process Knowledge/Wafer cleaning/RCA|RCA-clean]]) if the wafer is to be processed further.'''
KOH-etching is a highly versatile and cheap way to realize micro mechanical structures if you can live with the necessary Si<sub>3</sub>N<sub>4</sub>- or SiO<sub>2</sub>-masking materials and the potassium contamination of the surface. '''The latter necessitates in most cases a wet post-clean ([[Specific Process Knowledge/Wafer cleaning/7-up & Piranha|'7-up']] or [[Specific Process Knowledge/Wafer cleaning/RCA|RCA-clean]]) if the wafer is to be processed further. we also recommend to rinse the wafers in a 5% HCL solution to remove metal ions from the KOH solution.'''  


At Danchip we use as a standard a 28 wt% KOH. The etch rate - and the selectivity towards a SiO<sub>2</sub>-mask - is depending on the temperature. We normally use T=80 <sup>o</sup>C but may choose to reduce this to e.g. 60 <sup>o</sup>C or 70 <sup>o</sup>C in case of a high-precision timed etch (e.g. defining a thin membrane). In some cases we recommend to saturate the standard 28 wt% KOH with IPA with an etch temperature at T=70 <sup>o</sup>C (reduce evaporation of IPA). One example is for boron etch-stop, where the selectivity towards the boron-doped silicon is improved compared to the standard etch. Etching with IPA added to the KOH solution can be done in KOH fumehood.
At DTU Nanolab we use as a standard a 28 wt% KOH. The etch rate - and the selectivity towards a SiO<sub>2</sub>-mask - is depending on the temperature. We normally use T=80 <sup>o</sup>C but may choose to reduce this to e.g. 60 <sup>o</sup>C or 70 <sup>o</sup>C in case of a high-precision timed etch (e.g. defining a thin membrane). In some cases we recommend to saturate the standard 28 wt% KOH with IPA with an etch temperature at T=70 <sup>o</sup>C (reduce evaporation of IPA). One example is for boron etch-stop, where the selectivity towards the boron-doped silicon is improved compared to the standard etch. Etching with IPA added to the KOH solution (250ml IPA/1000ml KOH) can be done in KOH fumehood.  
   
   
<br clear="all" />
<br clear="all" />


<gallery caption="Different places to do anisotropic wet silicon etch" widths="300px" heights="200px" perrow="3">  
<gallery caption="Different places to do anisotropic wet silicon etch" widths="350px" heights="250px" perrow="3">  
image:KOH3_RR4_1.JPG|KOH3 bench for etch of 4" and 6" wafers. Positioned in cleanroom 4.  
image:KOH_BHF.JPG|Wetbench 01: Si etch, for Si etch of 4" and 6" wafers using KOH. Positioned in cleanroom D-3.  
image:KOH_4tommer.jpg|KOH etch for 4" wafers. KOH1 to the left and KOH2 to the right, in between you find the BHF tank. Positioned in cleanroom 3.
image:KOH_fumehood.JPG|Fume hood 06: Si etch, for Si etch of 4" and 6" wafers using KOH. Positioned in cleanroom D-3. This is used for wafers that are considered dirty. The workspace in the fume hood can also be booked and used for beaker etch of Si and in some cases Chromium etch.</gallery>
image:KOH_fumehood.JPG|KOH_fumehood is positioned in cleanroom 2. This is used for wafers that are considered dirty.</gallery>


Key facts for the different etch baths available at Danchip are resumed in the table:
'''The user manuals, quality control procedures and results, user APVs, technical information and contact information can be found in LabManager:'''
<!-- remember to remove the type of documents that are not present -->


<br clear="all" />


==KOH etching baths==
[http://labmanager.dtu.dk/function.php?module=Machine&view=view&mach=376 Si Etch 1: KOH info page in LabManager],
[http://labmanager.dtu.dk/function.php?module=Machine&view=view&mach=390 Si Etch 2: KOH info page in LabManager],
 
[http://labmanager.dtu.dk/function.php?module=Machine&view=view&mach=407 Si Etch 3: KOH info page in LabManager]


<br clear="all" />
==Process Information==


*[[/ProcessInfo#QC|QC info for standard KOH baths]]
*[[/ProcessInfo#Mixing KOH|How to mix KOH]]
*[[/ProcessInfo#Backside protection|Backside protection]]
*[[/ProcessInfo#Theory|Crystal orientation dependency]]


==KOH etching baths==
Key facts for the different etch baths available at DTU Nanolab are resumed in the table:
<br clear="all" />
{| border="2" cellspacing="0" cellpadding="2"  
{| border="2" cellspacing="0" cellpadding="2"  


!colspan="2" border="none" style="background:silver; color:black;" align="center"|Equipment  
!colspan="2" border="none" style="background:silver; color:black;" align="center"|Equipment  
|style="background:WhiteSmoke; color:black"|<b>KOH3</b>
|style="background:WhiteSmoke; color:black"|<b>Si Etch 01: KOH</b>
|style="background:WhiteSmoke; color:black"|<b>KOH2</b>
|style="background:WhiteSmoke; color:black"|<b>Si Etch 02: KOH</b>
|style="background:WhiteSmoke; color:black"|<b>KOH1</b>
|style="background:WhiteSmoke; color:black"|<b>Si Etch 03: KOH</b>
|style="background:WhiteSmoke; color:black"|<b>KOH Fumehood</b>
|-
|-
!style="background:silver; color:black;" align="center" width="60" rowspan="2"|Purpose  
!style="background:Silver; color:black;" align="center" width="60" rowspan="2"|Purpose  
|style="background:LightGrey; color:black"|Wet etch of Silicon
|style="background:LightGrey; color:black"|
|style="background:WhiteSmoke; color:black"|
*Etch of Silicon in 28 wt% KOH
*Etch of Silicon in 28 wt% KOH
|style="background:WhiteSmoke; color:black"|
|style="background:WhiteSmoke; color:black"|
Line 42: Line 57:
|style="background:WhiteSmoke; color:black"|
|style="background:WhiteSmoke; color:black"|
*Etch of Silicon in 28 wt% KOH  
*Etch of Silicon in 28 wt% KOH  
The bath is dedicated wafer with electroplated Nickel or otherwise dirty wafers
|style="background:WhiteSmoke; color:black"|
|style="background:WhiteSmoke; color:black"|
*Etch of Silicon in user mixed KOH
*Etch of Silicon in 28 wt% KOH
The bath is dedicated wafers with metal or otherwise dirty wafers
|-
|-
|style="background:LightGrey; color:black"|Link to safety APV and KBA
|style="background:LightGrey; color:black"|Link to safety APV and SDS
|style="background:WhiteSmoke; color:black"|
|style="background:WhiteSmoke; color:black"|
*:[http://labmanager.danchip.dtu.dk/d4Show.php?id=1906&mach=248 see APV here]
*:[http://labmanager.danchip.dtu.dk/d4Show.php?id=4964&mach=376 see APV here]
*:[http://kemibrug.dk/KBA/CAS/106882/?show_KBA=1&portaldesign=1 see KBA here]
*:[http://kemibrug.dk/KBA/CAS/106882/?show_KBA=1&portaldesign=1 see SDS here]
|style="background:WhiteSmoke; color:black"|
|style="background:WhiteSmoke; color:black"|
*:[http://labmanager.danchip.dtu.dk/d4Show.php?id=1906&mach=49 see APV here]
*:[http://labmanager.danchip.dtu.dk/d4Show.php?id=4964&mach=376 see APV here]
*:[http://kemibrug.dk/KBA/CAS/106882/?show_KBA=1&portaldesign=1 see KBA here]
*:[http://kemibrug.dk/KBA/CAS/106882/?show_KBA=1&portaldesign=1 see SDS here]
|style="background:WhiteSmoke; color:black"|
|style="background:WhiteSmoke; color:black"|
*:[http://labmanager.danchip.dtu.dk/d4Show.php?id=1906&mach=49 see APV here]
*:[http://labmanager.danchip.dtu.dk/d4Show.php?id=4897&mach=407 see APV here]
*:[http://kemibrug.dk/KBA/CAS/106882/?show_KBA=1&portaldesign=1 see KBA here]
*:[http://kemibrug.dk/KBA/CAS/106882/?show_KBA=1&portaldesign=1 see SDS here]
|style="background:WhiteSmoke; color:black"|
*:[http://labmanager.danchip.dtu.dk/d4Show.php?id=2479&mach=197 see APV here]
*:[http://kemibrug.dk/KBA/CAS/106882/?show_KBA=1&portaldesign=1 see KBA here]
|-
|-
!style="background:silver; color:black" align="center" valign="center" rowspan="4"|Performance
! rowspan="8" style="background:silver; color:black" align="center" valign="center" |Performance
|style="background:LightGrey; color:black"|Etch rates in crystalline silicon (100)
|style="background:LightGrey; color:black"|Etch rates in crystalline silicon (100)
|style="background:WhiteSmoke; color:black"|
|style="background:WhiteSmoke; color:black"|
Line 72: Line 84:
|style="background:WhiteSmoke; color:black"|
|style="background:WhiteSmoke; color:black"|
*0.4 µm/min (60 °C)
*0.4 µm/min (60 °C)
*0.7 µm/min (70 °C)
*1.3 µm/min (80 °C)
*1.3 µm/min (80 °C)
Etch rates might vary due to contamination and poor controlled concentration of the KOH solution
|-
|style="background:LightGrey; color:black"|Etch rates in crystalline silicon (110)
|style="background:WhiteSmoke; color:black"|
*2.5 µm/min (80 °C)
|style="background:WhiteSmoke; color:black"|
*2.5 µm/min (80 °C)
|style="background:WhiteSmoke; color:black"|
|style="background:WhiteSmoke; color:black"|
*Somewhat lower than in the dedicated baths. Approximately 1 µm/min @ 80 °C in 28 wt%
*2.5 µm/min (80 °C)
|-
|-
|style="background:LightGrey; color:black"|Etch rates in Thermal SiO2  
|style="background:LightGrey; color:black"|Etch rates in Thermal SiO2  
Line 81: Line 99:
*Theoretical values:
*Theoretical values:
*1.2 nm/min (60 °C)  
*1.2 nm/min (60 °C)  
*6 nm/min (80 °C)
*7.5 nm/min (80 °C)
|style="background:WhiteSmoke; color:black"|
|style="background:WhiteSmoke; color:black"|
*Theoretical values:
*Theoretical values:
*1.2 nm/min (60 °C)  
*1.2 nm/min (60 °C)  
*6 nm/min (80 °C)
*7.5 nm/min (80 °C)
|style="background:WhiteSmoke; color:black"|
|style="background:WhiteSmoke; color:black"|
*Theoretical values:
*1.2 nm/min (60 °C)
*7.5 nm/min (80 °C)
|-
|style="background:LightGrey; color:black"|Etch rates in other oxides
|style="background:WhiteSmoke; color:black"|
|style="background:WhiteSmoke; color:black"|
.
|style="background:WhiteSmoke; color:black"|
yannickseis@nbi.ku nov. 2017 @80 °C:
*BPSG from PECVD4: 311nm in about 3 min
*Waveguide oxide from PECVD4: 320nm etched in 26 min
*TEOS oxide from furnace: 300nm etched in 11 min
jemafh@nilt 2019-Marts:
*Standard from PECVD3: selectivity 1:100 to Si(100)
|style="background:WhiteSmoke; color:black"|
.
|-
|style="background:LightGrey; color:black"|Etch rates in PECVD SiN
|style="background:WhiteSmoke; color:black"|
|style="background:WhiteSmoke; color:black"|See etchrates for PECVD SiN [https://labadviser.nanolab.dtu.dk/index.php?title=Specific_Process_Knowledge/Thin_film_deposition/Deposition_of_Silicon_Nitride/Deposition_of_Silicon_Nitride_using_PECVD/PECVD3:_Low_stress_nitride_testing#DOE_made_to_find_a_good_QC_nitride_recipe_with_low_stress_and_low_KOH_etch_rate_(by_Berit_Herstrøm_@_DTU_Nanolab_2016_Marts) here]
|style="background:WhiteSmoke; color:black"|
|-
|style="background:LightGrey; color:black"|Etch rates in LPCVD Si3N4 and SiN
|style="background:WhiteSmoke; color:black"|
*Etch rates in LPCVD nitrides is very low. Etch selectivities to Si(100) is higher than 1:10.000
|style="background:WhiteSmoke; color:black"|
*Etch rates in LPCVD nitrides is very low. Etch selectivities to Si(100) is higher than 1:10.000
|style="background:WhiteSmoke; color:black"|
*Etch rates in LPCVD nitrides is very low. Etch selectivities to Si(100) is higher than 1:10.000
|-
|-
|style="background:LightGrey; color:black"|Roughness
|style="background:LightGrey; color:black"|Roughness
Line 96: Line 142:
|style="background:WhiteSmoke; color:black"|
|style="background:WhiteSmoke; color:black"|
*May be high due to contamination and poor controlled concentration of the KOH solution
*May be high due to contamination and poor controlled concentration of the KOH solution
|style="background:WhiteSmoke; color:black"|
*Typical worse than KOH2 and KOH3
|-
|-
|style="background:LightGrey; color:black"|Anisotropy
|style="background:LightGrey; color:black"|Anisotropy
|style="background:WhiteSmoke; color:black"|
*The etch rate is very dependent on the crystal orientation of the silicon.
|style="background:WhiteSmoke; color:black"|
|style="background:WhiteSmoke; color:black"|
*The etch rate is very dependent on the crystal orientation of the silicon.
*The etch rate is very dependent on the crystal orientation of the silicon.
Line 112: Line 154:
|style="background:LightGrey; color:black"|Chemical solution
|style="background:LightGrey; color:black"|Chemical solution
|style="background:WhiteSmoke; color:black"|
|style="background:WhiteSmoke; color:black"|
*28 wt% mixed in the ratio
*Mixing ratios giving 28 wt% KOH solutions
KOH:H<sub>2</sub>O - 500 g : 1000 ml
KOH:H<sub>2</sub>O - 1000 ml: 1200 ml, when using premixed 50% KOH solution
|style="background:WhiteSmoke; color:black"|
*28 wt% mixed in the ratio
KOH:H<sub>2</sub>O - 500 g : 1000 ml
|style="background:WhiteSmoke; color:black"|
|style="background:WhiteSmoke; color:black"|
*28 wt% mixed in the ratio
*Mixing ratios giving 28 wt% KOH solutions
KOH:H<sub>2</sub>O - 500 g : 1000 ml
KOH:H<sub>2</sub>O - 1000 ml: 1200 ml, when using premixed 50% KOH solution
|style="background:WhiteSmoke; color:black"|
|style="background:WhiteSmoke; color:black"|
*Custom made
*Mixing ratios giving 28 wt% KOH solutions
KOH:H<sub>2</sub>O - 1000 ml: 1200 ml, when using premixed 50% KOH solution
|-
|-
|style="background:LightGrey; color:black"|Temperature
|style="background:LightGrey; color:black"|Temperature
|style="background:WhiteSmoke; color:black"|
*Max 80 °C (standard etch)
|style="background:WhiteSmoke; color:black"|
|style="background:WhiteSmoke; color:black"|
*Max 80 °C (standard etch)
*Max 80 °C (standard etch)
Line 135: Line 173:
!style="background:silver; color:black" align="center" valign="center" rowspan="4"|Substrates
!style="background:silver; color:black" align="center" valign="center" rowspan="4"|Substrates
|style="background:LightGrey; color:black"|Batch size
|style="background:LightGrey; color:black"|Batch size
|style="background:WhiteSmoke; color:black"|
*1-25 wafers at a time
|style="background:WhiteSmoke; color:black"|
|style="background:WhiteSmoke; color:black"|
*1-25 wafers at a time  
*1-25 wafers at a time  
Line 146: Line 182:
|style="background:LightGrey; color:black"|Size of substrate
|style="background:LightGrey; color:black"|Size of substrate
|style="background:WhiteSmoke; color:black"|
|style="background:WhiteSmoke; color:black"|
*4” wafers
*4”-6" wafers
*6” wafers
|style="background:WhiteSmoke; color:black"|
|style="background:WhiteSmoke; color:black"|
*4” wafers
*4”-6" wafers
|style="background:WhiteSmoke; color:black"|
*4” wafers
|style="background:WhiteSmoke; color:black"|
|style="background:WhiteSmoke; color:black"|
*2” wafers
*2” wafers
*4” wafers
*4” wafers
*6” wafers
*Small pieces
*Small pieces
|-
|-
Line 166: Line 200:
*Silicon oxide  
*Silicon oxide  
*Silicon (oxy)nitride
*Silicon (oxy)nitride
|style="background:WhiteSmoke; color:black"|
*Silicon
*Silicon oxide
*Silicon (oxy)nitride
*Nickel
*Nickel vanadium alloys
*Titanium
*Chromium
*Gold
|style="background:WhiteSmoke; color:black"|
|style="background:WhiteSmoke; color:black"|
*All except for Polymers
*All except for Polymers
|-
|-
|style="background:LightGrey; color:black"|Masking material
|style="background:LightGrey; color:black"|Masking material
|style="background:WhiteSmoke; color:black"|
*Stoichiometric Si3N4
*Silicon rich nitride SiN
*PECVD Si3N4
*Thermal SiO2
|style="background:WhiteSmoke; color:black"|
|style="background:WhiteSmoke; color:black"|
*Stoichiometric Si3N4  
*Stoichiometric Si3N4  
Line 201: Line 221:
|-
|-
|}
|}
 
<sup>{{fn|1}}</sup> Measured by Eric Jensen from DTU-Nanotech, October 2013.
<br clear="all" />
<br clear="all" />
===Definition of structures===
Due to the almost inert (111)-planes it is possible by KOH etching to realize high aspect ratio structures in sigle crytalline silicon using the (111)-planes as sidewalls. In Si(100) these sidewalls are inclined - 54.7<sup>o</sup> with respect to the (100) surface - whereas in Si(110) the sidewalls are vertical (see figures below).
[[Image:KOH_Anisotropy.jpg|left|380px|thumb|Si(100)]]
[[Image:KOH_Anisotropy(110).jpg|380px|thumb|Si(110)]]
<br clear="all"/>
For Si(100), the relation between the width of the bottom of the etched groove (W<sub>b</sub>) and the width of the opening (W<sub>o</sub>) at the wafer surface in a groove etched to the depth l is given by:
<math>W_b = W_o - 2lcot(54.7^o) = W_o - \sqrt{2} l</math>
<br clear="all" />
===Definition of <110> alignment structures===
The etch rate dependence on the crystallographic planes can be used to determine the <110> crystal directions with high precision (better than +/- 0.05 <sup>o</sup>). A fast method for doing this, using the symmetric under-etching behavior around but not at the <110>-directions, was described by Vangbo and Bäcklund in J. Micromech. Microeng.'''6''' (1996), 279-284. High-precision control of the <110>-direction during alignment can be necessary in order to control the dimensions of KOH-etched structures (e.g. precise control of V-groove dimensions). A dedicated mask (MASK NAME) has been designed for this purpose.
<br clear="all" />
===Etch rates: Empirical formula (Seidl et al)===
The following empirical formula can be used for concentrations in the range of 10-60 wt%:
R = k<sub>0</sub> [H<sub>2</sub>O]<sup>4</sup> [KOH]<sup>0.25</sup> e<sup>-E<sub>a</sub>/kT</sup>,
where k<sub>0</sub> = 2480 µm/hr (mol/l)<sup>-4.25</sup>, E<sub>a</sub> = 0.595 eV for Si(100)
and  k<sub>0</sub> = 4500 µm/hr (mol/l)<sup>-4.25</sup>, E<sub>a</sub> = 0.60 eV for Si(110)

Latest revision as of 13:55, 15 September 2026

Feedback to this page: click here

Unless anything else is stated, everything on this page, text and pictures are made by DTU Nanolab.

All links to Kemibrug (SDS) and Labmanager Including APV and QC requires login.

Si etch - Anisotropic silicon etch

KOH belongs to the family of anisotropic Si-etchants based on aqueous alkaline solutions. The anisotropy stems from the different etch rates in different crystal directions. The {111}-planes are almost inert whereas the etch rates of e.g. {100}- and {110}-planes are several orders of magnitude faster.

KOH-etching is a highly versatile and cheap way to realize micro mechanical structures if you can live with the necessary Si3N4- or SiO2-masking materials and the potassium contamination of the surface. The latter necessitates in most cases a wet post-clean ('7-up' or RCA-clean) if the wafer is to be processed further. we also recommend to rinse the wafers in a 5% HCL solution to remove metal ions from the KOH solution.

At DTU Nanolab we use as a standard a 28 wt% KOH. The etch rate - and the selectivity towards a SiO2-mask - is depending on the temperature. We normally use T=80 oC but may choose to reduce this to e.g. 60 oC or 70 oC in case of a high-precision timed etch (e.g. defining a thin membrane). In some cases we recommend to saturate the standard 28 wt% KOH with IPA with an etch temperature at T=70 oC (reduce evaporation of IPA). One example is for boron etch-stop, where the selectivity towards the boron-doped silicon is improved compared to the standard etch. Etching with IPA added to the KOH solution (250ml IPA/1000ml KOH) can be done in KOH fumehood.


The user manuals, quality control procedures and results, user APVs, technical information and contact information can be found in LabManager:


Si Etch 1: KOH info page in LabManager,

Si Etch 2: KOH info page in LabManager,

Si Etch 3: KOH info page in LabManager

Process Information

KOH etching baths

Key facts for the different etch baths available at DTU Nanolab are resumed in the table:

Equipment Si Etch 01: KOH Si Etch 02: KOH Si Etch 03: KOH
Purpose
  • Etch of Silicon in 28 wt% KOH
  • Etch of Silicon in 28 wt% KOH
  • Etch of Silicon in 28 wt% KOH
  • Etch of Silicon in 28 wt% KOH

The bath is dedicated wafers with metal or otherwise dirty wafers

Link to safety APV and SDS
Performance Etch rates in crystalline silicon (100)
  • 0.4 µm/min (60 °C)
  • 0.7 µm/min (70 °C)
  • 1.3 µm/min (80 °C)
  • 0.4 µm/min (60 °C)
  • 0.7 µm/min (70 °C)
  • 1.3 µm/min (80 °C)
  • 0.4 µm/min (60 °C)
  • 0.7 µm/min (70 °C)
  • 1.3 µm/min (80 °C)
Etch rates in crystalline silicon (110)
  • 2.5 µm/min (80 °C)
  • 2.5 µm/min (80 °C)
  • 2.5 µm/min (80 °C)
Etch rates in Thermal SiO2
  • Theoretical values:
  • 1.2 nm/min (60 °C)
  • 7.5 nm/min (80 °C)
  • Theoretical values:
  • 1.2 nm/min (60 °C)
  • 7.5 nm/min (80 °C)
  • Theoretical values:
  • 1.2 nm/min (60 °C)
  • 7.5 nm/min (80 °C)
Etch rates in other oxides

.

yannickseis@nbi.ku nov. 2017 @80 °C:

  • BPSG from PECVD4: 311nm in about 3 min
  • Waveguide oxide from PECVD4: 320nm etched in 26 min
  • TEOS oxide from furnace: 300nm etched in 11 min

jemafh@nilt 2019-Marts:

  • Standard from PECVD3: selectivity 1:100 to Si(100)

.

Etch rates in PECVD SiN See etchrates for PECVD SiN here
Etch rates in LPCVD Si3N4 and SiN
  • Etch rates in LPCVD nitrides is very low. Etch selectivities to Si(100) is higher than 1:10.000
  • Etch rates in LPCVD nitrides is very low. Etch selectivities to Si(100) is higher than 1:10.000
  • Etch rates in LPCVD nitrides is very low. Etch selectivities to Si(100) is higher than 1:10.000
Roughness
  • Typical: 100-600 Å
  • Typical: 100-600 Å
  • May be high due to contamination and poor controlled concentration of the KOH solution
Anisotropy
  • The etch rate is very dependent on the crystal orientation of the silicon.
  • The etch rate is very dependent on the crystal orientation of the silicon.
  • The etch rate is very dependent on the crystal orientation of the silicon.
Process parameter range Chemical solution
  • Mixing ratios giving 28 wt% KOH solutions

KOH:H2O - 1000 ml: 1200 ml, when using premixed 50% KOH solution

  • Mixing ratios giving 28 wt% KOH solutions

KOH:H2O - 1000 ml: 1200 ml, when using premixed 50% KOH solution

  • Mixing ratios giving 28 wt% KOH solutions

KOH:H2O - 1000 ml: 1200 ml, when using premixed 50% KOH solution

Temperature
  • Max 80 °C (standard etch)
  • Max 80 °C
  • Max 80 °C
Substrates Batch size
  • 1-25 wafers at a time
  • 1-25 wafers at a time
  • 1-7 wafers at a time
Size of substrate
  • 4”-6" wafers
  • 4”-6" wafers
  • 2” wafers
  • 4” wafers
  • 6” wafers
  • Small pieces
Allowed materials
  • Silicon
  • Silicon oxide
  • Silicon (oxy)nitride
  • Silicon
  • Silicon oxide
  • Silicon (oxy)nitride
  • All except for Polymers
Masking material
  • Stoichiometric Si3N4
  • Silicon rich nitride SiN
  • PECVD Si3N4
  • Thermal SiO2
  • Stoichiometric Si3N4
  • Silicon rich nitride SiN
  • PECVD Si3N4
  • Thermal SiO2
  • Stoichiometric Si3N4
  • Silicon rich nitride SiN
  • PECVD Si3N4
  • Thermal SiO2

1 Measured by Eric Jensen from DTU-Nanotech, October 2013.