Specific Process Knowledge/Lithography/nLOF: Difference between revisions

From LabAdviser
Taran (talk | contribs)
Created page with "'''Feedback to this section''': '''[mailto:labadviser@danchip.dtu.dk?Subject=Feed%20back%20from%20page%20http://http://labadviser.danchip.dtu.dk/index.php/Specific_Process_Kno..."
 
Taran (talk | contribs)
 
(31 intermediate revisions by 2 users not shown)
Line 1: Line 1:
'''Feedback to this section''': '''[mailto:labadviser@danchip.dtu.dk?Subject=Feed%20back%20from%20page%20http://http://labadviser.danchip.dtu.dk/index.php/Specific_Process_Knowledge/Lithography/nLOF click here]'''
{{cc-nanolab}}


AZ nLOF 2020 is a negative UV photoresist, suitable for loft-off processes.
'''Feedback to this page''': '''[mailto:labadviser@nanolab.dtu.dk?Subject=Feed%20back%20from%20page%20http://labadviser.nanolab.dtu.dk/index.php/Specific_Process_Knowledge/Lithography/nLOF click here]'''
 
[[Category: Lithography|Resist]]
[[Category: Resist|AZ nLOF 2020]]
 
__TOC__
 
==Resist description==
AZ nLOF 2020 is a negative UV photoresist, suitable for lift-off processes.
 
==Spin coating==
[[Image:nLOFspincurves.JPG|500x500px|thumb|Spin curves for AZ nLOF 2020 using a 30s spin-off, and a 60s@110°C softbake]]
 
'''Typical spin parameters:'''
*Spin off: 30-60 s
*Soft bake: 60 s @ 110°C
 
<br clear="all" />


==Post-exposure bake==
==Post-exposure bake==
'''Typical PEB parameters:'''
*PEB temperature: 110°C
*PEB time: 60 s
The manufacturer recommended PEB for nLOF is 60 seconds at 110°C, regardless of resist film thickness. 


The recommended PEB for nLOF is 60s at 110°C, regardless of resist film thickness.
===PEB baking time investigation===
While 60 s @ 110°C is adequate for Si substrates, less thermally conductive substrates (glass, III-V materials, chips bonded to carrier), have shown problems using the standard PEB recipe.<br>
These problems were largely solved by increasing the PEB time to 120 s. Tests (on Aligner: Maskless 02) have shown that the lithographic performance of nLOF on Si is improved when using 120 s @ 110°C PEB (less stitching, less bias, more negative profile).  


While 1min@110°C is adequate for Si substrates, less thermally conductive substrates (glass, III-V materials, chips bonded to carrier), have shoved problems using the standard PEB. These problems were largely solved by increasing the PEB time to 2min. Tests (on Aligner: Maskless 02) have shown that the lithographic performance of nLOF on Si is improved by using 2min@110°C PEB (less stitching, less bias, more negative profile).
A small report on the tests can be found here: [[media:nLOF_PEBtime_2019.pdf|'''nLOF PEB time 2019''']].


==Development==
==Development==
'''Development speed:'''
*Puddle development in 2.38% TMAH (AZ 726 MIF): ~4 µm/min
A 2 µm nLOF resist film is fully developed in ~30 s in 2.38% TMAH (AZ 726 MIF). However, the development can be continued to 60 s in order to get a more negative resist profile (due to increased under-cut).
===Solvent development===
Cross-linking negative resists have the potential to be developed using organic solvents instead of the normally used alkaline aqueous solutions. A quick test of this was carried out by Thomas Anhøj @ DTU Nanolab, showing that nLOF 2020 could potentially be used for water-free lithography.


A 2µm nLOF resist film is fully developed in 20-30s using TMAH (AZ 726). However, the development can be continued to 60s in order to get a nore negative resist profile (increase the under-cut).
A small report on the test can be found here: [[media:nLOF_solventdev_2024.pdf|'''nLOF solvent development 2024''']].

Latest revision as of 11:22, 30 October 2026

The content on this page, including all images and pictures, was created by DTU Nanolab staff, unless otherwise stated.

Feedback to this page: click here

Resist description

AZ nLOF 2020 is a negative UV photoresist, suitable for lift-off processes.

Spin coating

Spin curves for AZ nLOF 2020 using a 30s spin-off, and a 60s@110°C softbake

Typical spin parameters:

  • Spin off: 30-60 s
  • Soft bake: 60 s @ 110°C


Post-exposure bake

Typical PEB parameters:

  • PEB temperature: 110°C
  • PEB time: 60 s

The manufacturer recommended PEB for nLOF is 60 seconds at 110°C, regardless of resist film thickness.

PEB baking time investigation

While 60 s @ 110°C is adequate for Si substrates, less thermally conductive substrates (glass, III-V materials, chips bonded to carrier), have shown problems using the standard PEB recipe.
These problems were largely solved by increasing the PEB time to 120 s. Tests (on Aligner: Maskless 02) have shown that the lithographic performance of nLOF on Si is improved when using 120 s @ 110°C PEB (less stitching, less bias, more negative profile).

A small report on the tests can be found here: nLOF PEB time 2019.

Development

Development speed:

  • Puddle development in 2.38% TMAH (AZ 726 MIF): ~4 µm/min

A 2 µm nLOF resist film is fully developed in ~30 s in 2.38% TMAH (AZ 726 MIF). However, the development can be continued to 60 s in order to get a more negative resist profile (due to increased under-cut).

Solvent development

Cross-linking negative resists have the potential to be developed using organic solvents instead of the normally used alkaline aqueous solutions. A quick test of this was carried out by Thomas Anhøj @ DTU Nanolab, showing that nLOF 2020 could potentially be used for water-free lithography.

A small report on the test can be found here: nLOF solvent development 2024.