Specific Process Knowledge/Etch/Wet Gold Etch: Difference between revisions
No edit summary |
|||
| (10 intermediate revisions by 5 users not shown) | |||
| Line 1: | Line 1: | ||
'''Feedback to this page''': '''[mailto:wetchemistry@ | '''Feedback to this page''': '''[mailto:wetchemistry@nanolab.dtu.dk?Subject=Feed%20back%20from%20page%20http://labadviser.nanolab.dtu.dk/index.php/Specific_Process_Knowledge/Etch/Wet_Gold_Etch click here]''' | ||
'''Unless anything else is stated, everything on this page text and pictures are made by DTU Nanolab.''' | |||
'''All links to Kemibrug (SDS) and Labmanager Including APV requires login.''' | |||
'''All measurements on this page has been made by Nanolab staff.''' | |||
[[Category:Equipment|Etch Wet Gold]] | |||
[[Category:Etch (Wet) bath|Gold]] | |||
Ething of Gold can be done either wet or dry. For wet etching please see below on this page. Dry etching can be done with [[Specific Process Knowledge/Etch/IBE⁄IBSD Ionfab 300|IBE]] by sputtering with Ar ions. | Ething of Gold can be done either wet or dry. For wet etching please see below on this page. Dry etching can be done with [[Specific Process Knowledge/Etch/IBE⁄IBSD Ionfab 300|IBE]] by sputtering with Ar ions. | ||
| Line 5: | Line 14: | ||
==Etching of Gold== | ==Etching of Gold== | ||
[[Image: | [[Image:Fumehood1-2.jpg |300x300px|thumb|Wet Gold Etch can be done in Fumehood 1 or 2 in cleanroom D-3]] | ||
Wet etching of gold is done making your own set up using a beaker in a fumehood. You can see the APV [http://labmanager.dtu.dk/d4Show.php?id=4748&mach=368 here]. | |||
We have two different solutions: | We have two different solutions: | ||
# Iodine etch: KI:I<sub>2</sub>:H<sub>2</sub>O - 100g:25g:500ml - standard at | # Iodine etch: KI:I<sub>2</sub>:H<sub>2</sub>O - 100g:25g:500ml - standard at DTU Nanolab. Can be used with AZ resist as mask. | ||
# Aqua Regia (Kongevand): HNO<sub>3</sub>:HCl - 1:3 - A very strong acid which will etch most metals and | # Aqua Regia (Kongevand): HNO<sub>3</sub>:HCl - 1:3 - A very strong acid which will etch most metals and is therefore used when you wish to remove all the gold from your wafer. '''You must be very careful when working with Aqua Regia (Kongevand). It can generate nitrogen oxide gases which are very toxic!''' | ||
| Line 23: | Line 32: | ||
! | ! | ||
! Iodine based gold etch | ! Iodine based gold etch | ||
! Aqua Regia ( | ! Aqua Regia (kongevand) | ||
! Dilute Aqua Regia (fortyndet kongevand) | |||
|- | |- | ||
| Line 30: | Line 40: | ||
!General description | !General description | ||
| | | | ||
Etch of | Etch of gold with or without photoresist mask. | ||
| | | | ||
Etch of | Etch of gold (as stripper). | ||
| | |||
Etch of gold. | |||
|- | |- | ||
|-style="background:LightGrey; color:black" | |-style="background:LightGrey; color:black" | ||
!Link to safety APV | !Link to safety APV | ||
|[http://labmanager | |[http://labmanager.dtu.dk/d4Show.php?id=4748&mach=368 See APV here]. | ||
|[http://labmanager. | |[http://labmanager.dtu.dk/d4Show.php?id=4748&mach=368 See APV here] | ||
|[http://labmanager.dtu.dk/d4Show.php?id=4748&mach=368 See APV here] | |||
|- | |- | ||
| Line 46: | Line 59: | ||
|KI:I<sub>2</sub>:H<sub>2</sub>O (100g:25g:500ml) | |KI:I<sub>2</sub>:H<sub>2</sub>O (100g:25g:500ml) | ||
|HCl:HNO<sub>3</sub> (3:1) | |HCl:HNO<sub>3</sub> (3:1) | ||
|HCl:HNO<sub>3</sub>:H<sub>2</sub>O (3:1:2) | |||
|- | |- | ||
| Line 51: | Line 65: | ||
|-style="background:LightGrey; color:black" | |-style="background:LightGrey; color:black" | ||
!Process temperature | !Process temperature | ||
| | |20°C | ||
| | |20°C | ||
|20-30°C | |||
|- | |- | ||
| Line 64: | Line 79: | ||
| | | | ||
Unmasked - used as a stripper | Unmasked - used as a stripper | ||
| | |||
Difficult to mask. Mainly used as a stripper. | |||
|- | |- | ||
| Line 73: | Line 90: | ||
| | | | ||
~(??) nm/min - fast etch | ~(??) nm/min - fast etch | ||
| | |||
~680 nm/min at 30°C | |||
|- | |- | ||
| Line 79: | Line 98: | ||
!Batch size | !Batch size | ||
| | | | ||
1-5 | 1-5 4" wafers at a time | ||
| | | | ||
1-5 4" | 1-5 4" wafers at a time | ||
| | |||
1-5 4" wafers at a time | |||
|- | |- | ||
| Line 87: | Line 108: | ||
|-style="background:LightGrey; color:black" | |-style="background:LightGrey; color:black" | ||
!Size of substrate | !Size of substrate | ||
|Any size and number that can go inside the beaker in use | |||
|Any size and number that can go inside the beaker in use | |Any size and number that can go inside the beaker in use | ||
|Any size and number that can go inside the beaker in use | |Any size and number that can go inside the beaker in use | ||
| Line 98: | Line 120: | ||
| | | | ||
No restrictions when used in beaker. | No restrictions when used in beaker. | ||
Make a note on the beaker of which materials have been processed. | |||
| | |||
No restrictions when used in beaker. | |||
Make a note on the beaker of which materials have been processed. | Make a note on the beaker of which materials have been processed. | ||
|- | |- | ||
|} | |} | ||
Latest revision as of 13:40, 15 September 2026
Feedback to this page: click here
Unless anything else is stated, everything on this page text and pictures are made by DTU Nanolab.
All links to Kemibrug (SDS) and Labmanager Including APV requires login.
All measurements on this page has been made by Nanolab staff.
Ething of Gold can be done either wet or dry. For wet etching please see below on this page. Dry etching can be done with IBE by sputtering with Ar ions.
Etching of Gold

Wet etching of gold is done making your own set up using a beaker in a fumehood. You can see the APV here.
We have two different solutions:
- Iodine etch: KI:I2:H2O - 100g:25g:500ml - standard at DTU Nanolab. Can be used with AZ resist as mask.
- Aqua Regia (Kongevand): HNO3:HCl - 1:3 - A very strong acid which will etch most metals and is therefore used when you wish to remove all the gold from your wafer. You must be very careful when working with Aqua Regia (Kongevand). It can generate nitrogen oxide gases which are very toxic!
Comparing the two solutions
| Iodine based gold etch | Aqua Regia (kongevand) | Dilute Aqua Regia (fortyndet kongevand) | |
|---|---|---|---|
| General description |
Etch of gold with or without photoresist mask. |
Etch of gold (as stripper). |
Etch of gold. |
| Link to safety APV | See APV here. | See APV here | See APV here |
| Chemical solution | KI:I2:H2O (100g:25g:500ml) | HCl:HNO3 (3:1) | HCl:HNO3:H2O (3:1:2) |
| Process temperature | 20°C | 20°C | 20-30°C |
| Possible masking materials |
Photoresist (1.5 µm AZ5214E) |
Unmasked - used as a stripper |
Difficult to mask. Mainly used as a stripper. |
| Etch rate |
~100 nm/min |
~(??) nm/min - fast etch |
~680 nm/min at 30°C |
| Batch size |
1-5 4" wafers at a time |
1-5 4" wafers at a time |
1-5 4" wafers at a time |
| Size of substrate | Any size and number that can go inside the beaker in use | Any size and number that can go inside the beaker in use | Any size and number that can go inside the beaker in use |
| Allowed materials |
No restrictions when used in beaker. Make a note on the beaker of which materials have been processed. |
No restrictions when used in beaker. Make a note on the beaker of which materials have been processed. |
No restrictions when used in beaker. Make a note on the beaker of which materials have been processed. |