Specific Process Knowledge/Lithography/Aligners/MAvsMLA: Difference between revisions
| (23 intermediate revisions by the same user not shown) | |||
| Line 1: | Line 1: | ||
{{cc-nanolab}} | {{cc-nanolab}} | ||
'''Feedback to this page''': '''[mailto: | '''Feedback to this page''': '''[mailto:taran@nanolab.dtu.dk?Subject=Feed%20back%20from%20page%20http://labadviser.nanolab.dtu.dk/index.php?title=Specific_Process_Knowledge/Lithography/Aligners/MAvsMLA click here]''' | ||
[[Category:Equipment|Lithography exposure]] | [[Category:Equipment|Lithography exposure]] | ||
| Line 10: | Line 10: | ||
=Mask Aligner vs Maskless Aligner= | =Mask Aligner vs Maskless Aligner= | ||
Slides presented at NNUM in Uppsala | In the first half of 2026, a rather thorough investigation of the differences between exposure using mask aligner and maskless aligner was conducted. The result was presented as an advanced lithography tutorial at the 2026 Nordic Nanolab User Meeting in Uppsala, Sweden. | ||
Slides presented at NNUM in Uppsala: [[Media:MA6 vs MLA 2026 v09.pdf|'''MA6 vs MLA 2026_v09''']] | |||
Mask design used in the investigation: [[Media:LithoTestAlign 2025 v10.gds|LithoTestAlign_2025_v10.gds]] | Mask design used in the investigation: [[Media:LithoTestAlign 2025 v10.gds|LithoTestAlign_2025_v10.gds]] | ||
<br clear="all" /> | |||
=Tools used in the investigation= | |||
*Wafers | |||
**100mm Si, SSP <100> | |||
*Resists | |||
**[[Specific_Process_Knowledge/Lithography/5214E|AZ 5214E]] (image reversal resist, but processed positive) | |||
**[[Specific_Process_Knowledge/Lithography/MiR|AZ MiR 701]] (positive tone resist) | |||
**[[Specific_Process_Knowledge/Lithography/nLOF|AZ nLOF 2020]] (negative tone resist) | |||
*Spin coating (incl. HMDS) | |||
**[[Specific_Process_Knowledge/Lithography/Coaters#Spin_Coater:_Gamma_UV|Spin Coater: Gamma UV]] | |||
*Exposure | |||
**[[Specific_Process_Knowledge/Lithography/UVExposure/aligner_MA6-2|Aligner: MA6-2]] | |||
**[[Specific_Process_Knowledge/Lithography/UVExposure/aligner_MA6-1|Aligner: MA6-1]] (in PolyFabLab) | |||
**[[Specific Process Knowledge/Lithography/UVExposure/aligner_MLA2|Aligner: Maskless 02]] | |||
**[[Specific Process Knowledge/Lithography/UVExposure/aligner_MLA1|Aligner: Maskless 01]] | |||
*Development (incl. PEB, if relevant) | |||
**[[Specific_Process_Knowledge/Lithography/Development/UV_developer|Developer: TMAH UV-lithography]] | |||
*Inspection | |||
**[[Specific_Process_Knowledge/Characterization/Optical_microscope|Microscope Olympus MX63]] | |||
**[[Specific_Process_Knowledge/Characterization/SEM_Supra_1|SEM Supra 1]] | |||
**[[Specific_Process_Knowledge/Characterization/SEM_Supra_3|SEM Supra 3]] | |||
<br clear="all" /> | |||
=Data from the investigation= | =Data from the investigation= | ||
<span style="background:#FF2800">THIS PAGE IS UNDER CONSTRUCTION</span>[[image:Under_construction.png|200px]] | <!-- <span style="background:#FF2800">THIS PAGE IS UNDER CONSTRUCTION</span>[[image:Under_construction.png|200px]] | ||
--> | |||
==AZ 5214E== | <br clear="all" /> | ||
==AZ 5214E== | |||
<br clear="all" /> | |||
===Resolution (AZ 5214E)=== | ===Resolution (AZ 5214E)=== | ||
<br clear="all" /> | <br clear="all" /> | ||
| Line 191: | Line 218: | ||
===Resist profile (AZ 5214E)=== | ===Resist profile (AZ 5214E)=== | ||
<br clear="all" /> | <br clear="all" /> | ||
====Linewidth and sidewall angle vs exposure dose (AZ 5214E)==== | ====Linewidth and sidewall angle vs exposure dose (AZ 5214E)==== | ||
<br clear="all" /> | <br clear="all" /> | ||
'''Result of image analysis of SEM images of 2µm triplets:''' | '''Result of image analysis of SEM images of 2µm triplets:''' | ||
| Line 282: | Line 307: | ||
====Linewidth and sidewall angle vs defocus parameter (AZ 5214E)==== | ====Linewidth and sidewall angle vs defocus parameter (AZ 5214E)==== | ||
<br clear="all" /> | <br clear="all" /> | ||
'''Result of image analysis of SEM images of 2µm triplets:''' | |||
{| cellpadding="2" style="border: 2px solid darkgray;" align="left" | |||
! width="510" | | |||
|+ | |||
|- border="0" align="center" | |||
|[[Image:5214E_Profile vs defoc.jpg|500px]] | |||
|- align="center" | |||
| Linewidth and sidewall angle vs. defocus value for 1.5µm AZ 5214E exposed in Aligner: Maskless 02 (MLA2) using dose 95mJ/cm<sup>2</sup>. <br>Blue circles: Width of 2µm line. <br>Orange Squares: Sidewall angle. | |||
|} | |||
<br clear="all" /> | |||
'''SEM images of 1.5µm AZ 5214E as a function of defocus parameter for Aligner: Maskless 02 (MLA2) using dose 95mJ/cm<sup>2</sup>:''' | '''SEM images of 1.5µm AZ 5214E as a function of defocus parameter for Aligner: Maskless 02 (MLA2) using dose 95mJ/cm<sup>2</sup>:''' | ||
{|border="1" cellspacing="0" cellpadding="3" style="text-align:left;" | {|border="1" cellspacing="0" cellpadding="3" style="text-align:left;" | ||
|- | |- | ||
| Line 318: | Line 359: | ||
<br clear="all" /> | <br clear="all" /> | ||
==AZ MiR 701== | |||
<br clear="all" /> | <br clear="all" /> | ||
===Resolution (AZ MiR 701)=== | ===Resolution (AZ MiR 701)=== | ||
<br clear="all" /> | |||
'''Resolution at optimal processing conditions for 1.5µm AZ MiR 701 using different exposure equipment:''' | '''Resolution at optimal processing conditions for 1.5µm AZ MiR 701 using different exposure equipment:''' | ||
{| class="wikitable" | {| class="wikitable" | ||
| Line 396: | Line 423: | ||
====Linewidth and sidewall angle vs exposure dose (AZ MiR 701)==== | ====Linewidth and sidewall angle vs exposure dose (AZ MiR 701)==== | ||
<br clear="all" /> | <br clear="all" /> | ||
'''Result of image analysis of SEM images of 2µm triplets:''' | |||
{| cellpadding="2" style="border: 2px solid darkgray;" align="left" | |||
! width="510" | | |||
|+ | |||
|- border="0" align="center" | |||
|[[Image:MiR_Linewidth vs dose.jpg|500px]] | |||
|[[Image:MiR_Sidewall vs dose.jpg|500px]] | |||
|- align="center" | |||
| colspan="2" | Width of 2µm line and sidewall angle vs. exposure dose for 1.5µm AZ MiR 701. <br>Blue circles: Exposed on Aligner: MA6-2 in vacuum contact. <br>Orange Squares: Exposed on Aligner: Maskless 02 (MLA2) using defoc 2 (QC defoc=2). | |||
|} | |||
<br clear="all" /> | |||
'''SEM images of 1.5µm AZ MiR 701 as a function of exposure dose for Aligner: MA6-2 using vacuum contact:''' | '''SEM images of 1.5µm AZ MiR 701 as a function of exposure dose for Aligner: MA6-2 using vacuum contact:''' | ||
| Line 414: | Line 457: | ||
|-style="background:WhiteSmoke; color:black" | |-style="background:WhiteSmoke; color:black" | ||
|2µm triplets | |2µm triplets | ||
|[[Image:W18 MA62 MiR vac | |[[Image:W18 MA62 MiR vac D160_F8T_04.jpg|280px]] | ||
|[[Image:W18 MA62 MiR vac D190_H6B_03.jpg|280px]] | |[[Image:W18 MA62 MiR vac D190_H6B_03.jpg|280px]] | ||
|[[Image:W18 MA62 MiR vac D220_I3T_03.jpg|280px]] | |[[Image:W18 MA62 MiR vac D220_I3T_03.jpg|280px]] | ||
| Line 462: | Line 505: | ||
|} | |} | ||
<br clear="all" /> | |||
====Linewidth and sidewall angle vs defocus parameter (AZ MiR 701)==== | |||
<br clear="all" /> | <br clear="all" /> | ||
'''Result of image analysis of SEM images of 2µm triplets:''' | '''Result of image analysis of SEM images of 2µm triplets:''' | ||
{| cellpadding="2" style="border: 2px solid darkgray;" align="left" | {| cellpadding="2" style="border: 2px solid darkgray;" align="left" | ||
! width="510" | | ! width="510" | | ||
|+ | |+ | ||
|- border="0" align="center" | |- border="0" align="center" | ||
|[[Image: | |[[Image:MiR_Profile vs defoc.jpg|500px]] | ||
|- align="center" | |- align="center" | ||
| | | Linewidth and sidewall angle vs. defocus value for 1.5µm AZ MiR 701 exposed in Aligner: Maskless 02 (MLA2) using dose 95mJ/cm<sup>2</sup>. <br>Blue circles: Width of 2µm line. <br>Orange Squares: Sidewall angle. | ||
|} | |} | ||
<br clear="all" /> | <br clear="all" /> | ||
'''SEM images of 1.5µm AZ MiR 701 as a function of defocus parameter for Aligner: Maskless 02 (MLA2) using dose 275mJ/cm<sup>2</sup>:''' | '''SEM images of 1.5µm AZ MiR 701 as a function of defocus parameter for Aligner: Maskless 02 (MLA2) using dose 275mJ/cm<sup>2</sup>:''' | ||
| Line 517: | Line 560: | ||
<br clear="all" /> | <br clear="all" /> | ||
==AZ nLOF 2020== | |||
<br clear="all" /> | <br clear="all" /> | ||
===Resolution (AZ nLOF 2020)=== | ===Resolution (AZ nLOF 2020)=== | ||
<br clear="all" /> | <br clear="all" /> | ||
'''Resolution at optimal processing conditions for 2µm AZ nLOF 2020 using different exposure equipment:''' | '''Resolution at optimal processing conditions for 2µm AZ nLOF 2020 using different exposure equipment:''' | ||
{| class="wikitable" | {| class="wikitable" | ||
| Line 582: | Line 611: | ||
154mJ/cm<sup>2</sup>, vacuum contact | 154mJ/cm<sup>2</sup>, vacuum contact | ||
|[[Image:W07 MA6 nLOF D154 vac C8T_01.jpg|400px]] | |[[Image:W07 MA6 nLOF D154 vac C8T_01.jpg|400px]] | ||
|[[Image:W07 MA6 nLOF D154 vac | |[[Image:W07 MA6 nLOF D154 vac C8T_03.jpg|400px]] | ||
|[[Image:W07 MA6 nLOF D154 vac | |[[Image:W07 MA6 nLOF D154 vac C8T_04.jpg|400px]] | ||
|- | |- | ||
| Line 589: | Line 618: | ||
|Aligner: Maskless 01 (MLA1) | |Aligner: Maskless 01 (MLA1) | ||
220mJ/cm<sup>2</sup>, Defoc -4 | 220mJ/cm<sup>2</sup>, Defoc -4 | ||
|[[Image:W06 MLA1 nLOF D220 F- | |[[Image:W06 MLA1 nLOF D220 F-4_2_01.jpg|400px]] | ||
|[[Image:W06 MLA1 nLOF D220 F- | |[[Image:W06 MLA1 nLOF D220 F-4_2_03.jpg|400px]] | ||
|[[Image:W06 MLA1 nLOF D220 F- | |[[Image:W06 MLA1 nLOF D220 F-4_2_04.jpg|400px]] | ||
|- | |- | ||
| Line 598: | Line 627: | ||
450mJ/cm<sup>2</sup>, defoc 0 | 450mJ/cm<sup>2</sup>, defoc 0 | ||
|[[Image:W17 mla2 nLOF D450 F0_04.jpg|400px]] | |[[Image:W17 mla2 nLOF D450 F0_04.jpg|400px]] | ||
|[[Image:W17 mla2 nLOF D450 | |[[Image:W17 mla2 nLOF D450 F0_03.jpg|400px]] | ||
|[[Image:W17 mla2 nLOF D450 | |[[Image:W17 mla2 nLOF D450 F0_02.jpg|400px]] | ||
|} | |} | ||
| Line 630: | Line 659: | ||
220mJ/cm<sup>2</sup>, Defoc -4 | 220mJ/cm<sup>2</sup>, Defoc -4 | ||
|[[Image:W06 MLA1 nLOF D220 F-4_02.jpg|400px]] | |[[Image:W06 MLA1 nLOF D220 F-4_02.jpg|400px]] | ||
|[[Image:W06 MLA1 nLOF D220 F- | |[[Image:W06 MLA1 nLOF D220 F-4_2_01.jpg|400px]] | ||
|[[Image:W06 MLA1 nLOF D220 F-4_03.jpg|400px]] | |[[Image:W06 MLA1 nLOF D220 F-4_03.jpg|400px]] | ||
| Line 653: | Line 682: | ||
|Aligner: Maskless 01 (MLA1) | |Aligner: Maskless 01 (MLA1) | ||
220mJ/cm<sup>2</sup>, Defoc -4 | 220mJ/cm<sup>2</sup>, Defoc -4 | ||
|[[Image:w04_mla1_nLOF_D220_F-4_X_l_2um.jpg| | |[[Image:w04_mla1_nLOF_D220_F-4_X_l_2um.jpg|340px]] | ||
|[[Image:w04_mla1_nLOF_D220_F-4_X_t_2um.jpg| | |[[Image:w04_mla1_nLOF_D220_F-4_X_t_2um.jpg|340px]] | ||
|[[Image:w04_mla1_nLOF_D220_F-4_Xlines.jpg| | |[[Image:w04_mla1_nLOF_D220_F-4_Xlines.jpg|340px]] | ||
|[[Image:w04_mla1_nLOF_D220_F-4_Xtrench.jpg| | |[[Image:w04_mla1_nLOF_D220_F-4_Xtrench.jpg|340px]] | ||
|} | |} | ||
| Line 662: | Line 691: | ||
===Resist profile (AZ nLOF 2020)=== | ===Resist profile (AZ nLOF 2020)=== | ||
<br clear="all" /> | |||
====Linewidth and sidewall angle vs exposure dose (AZ nLOF 2020)==== | |||
<br clear="all" /> | |||
'''Result of image analysis of SEM images of 2µm triplets:''' | '''Result of image analysis of SEM images of 2µm triplets:''' | ||
| Line 679: | Line 709: | ||
<br clear="all" /> | <br clear="all" /> | ||
'''SEM images of 2µm AZ nLOF 2020 as a function of exposure dose for Aligner: MA6-2 using vacuum contact:''' | |||
{|border="1" cellspacing="0" cellpadding="3" style="text-align:left;" | |||
|- | |||
|- | |||
|-style="background:silver; color:black" | |||
! | |||
!100mJ/cm<sup>2</sup> | |||
!120mJ/cm<sup>2</sup> | |||
!140mJ/cm<sup>2</sup> | |||
!160mJ/cm<sup>2</sup> | |||
|- | |||
|- | |||
|-style="background:WhiteSmoke; color:black" | |||
|2µm triplets | |||
|[[Image:w05_ma6_nLOF_D100_vac_2um.jpg|340px]] | |||
|[[Image:w05_ma6_nLOF_D120_vac_2um.jpg|340px]] | |||
|[[Image:w05_ma6_nLOF_D140_vac_2um.jpg|340px]] | |||
|[[Image:w05_ma6_nLOF_D160_vac_2um.jpg|340px]] | |||
|} | |||
<br clear="all" /> | |||
'''SEM images of 2µm AZ nLOF 2020 as a function of exposure dose for Aligner: Maskless 01 (MLA1) using defoc -4:''' | |||
{|border="1" cellspacing="0" cellpadding="3" style="text-align:left;" | |||
|- | |||
|- | |||
|-style="background:silver; color:black" | |||
! | |||
!200mJ/cm<sup>2</sup> | |||
!220mJ/cm<sup>2</sup> | |||
!240mJ/cm<sup>2</sup> | |||
|- | |||
|- | |||
|-style="background:WhiteSmoke; color:black" | |||
|2µm triplets | |||
|[[Image:w04_mla1_nLOF_D200_F-4_2um.jpg|340px]] | |||
|[[Image:w04_mla1_nLOF_D220_F-4_2um.jpg|340px]] | |||
|[[Image:w04_mla1_nLOF_D240_F-4_2um.jpg|340px]] | |||
|} | |||
<br clear="all" /> | |||
'''SEM images of 2µm AZ nLOF 2020 as a function of exposure dose for Aligner: Maskless 02 (MLA2) using defoc 0:''' | |||
{|border="1" cellspacing="0" cellpadding="3" style="text-align:left;" | |||
|- | |||
|- | |||
|-style="background:silver; color:black" | |||
! | |||
!400mJ/cm<sup>2</sup> | |||
!450mJ/cm<sup>2</sup> | |||
!500mJ/cm<sup>2</sup> | |||
|- | |||
|- | |||
|-style="background:WhiteSmoke; color:black" | |||
|2µm triplets | |||
|[[Image:W17 mla2 nLOF D400 F0_01.jpg|340px]] | |||
|[[Image:W17 mla2 nLOF D450 F0_04.jpg|340px]] | |||
|[[Image:W17 mla2 nLOF D500 F0_01.jpg|340px]] | |||
|} | |||
<br clear="all" /> | |||
====Linewidth and sidewall angle vs defocus parameter (AZ nLOF 2020)==== | |||
<br clear="all" /> | |||
'''Result of image analysis of SEM images of 2µm triplets:''' | '''Result of image analysis of SEM images of 2µm triplets:''' | ||
| Line 691: | Line 794: | ||
|- align="center" | |- align="center" | ||
| colspan="2" | Linewidth and sidewall angle vs. defocus value for 2µm AZ nLOF <br>exposed in Aligner: Maskless 01 (MLA1) using dose 220mJ/cm<sup>2</sup> and Aligner: Maskless 02 (MLA2) using dose 450mJ/cm<sup>2</sup>, respectively. <br>Blue circles: Width of 2µm line. Orange Squares: Sidewall angle. | | colspan="2" | Linewidth and sidewall angle vs. defocus value for 2µm AZ nLOF <br>exposed in Aligner: Maskless 01 (MLA1) using dose 220mJ/cm<sup>2</sup> and Aligner: Maskless 02 (MLA2) using dose 450mJ/cm<sup>2</sup>, respectively. <br>Blue circles: Width of 2µm line. Orange Squares: Sidewall angle. | ||
|} | |||
<br clear="all" /> | |||
'''SEM images of 2µm AZ nLOF 2020 as a function of defocus parameter for Aligner: Maskless 01 (MLA1) using dose 220mJ/cm<sup>2</sup>:''' | |||
{|border="1" cellspacing="0" cellpadding="3" style="text-align:left;" | |||
|- | |||
|- | |||
|-style="background:silver; color:black" | |||
! | |||
!Defoc -14 | |||
!Defoc -7 | |||
!Defoc -4 | |||
!Defoc -1 | |||
!Defoc -6 | |||
|- | |||
|- | |||
|-style="background:WhiteSmoke; color:black" | |||
|2µm triplets | |||
|[[Image:W06 MLA1 nLOF D220 F-14_02.jpg|280px]] | |||
|[[Image:W06 MLA1 nLOF D220 F-7_01.jpg|280px]] | |||
|[[Image:W06 MLA1 nLOF D220 F-4_2_01.jpg|280px]] | |||
|[[Image:W06 MLA1 nLOF D220 F-1_01.jpg|280px]] | |||
|[[Image:W06 MLA1 nLOF D220 F6_02.jpg|280px]] | |||
|- | |||
|-style="background:WhiteSmoke; color:black" | |||
|Lines | |||
|[[Image:W06 MLA1 nLOF D220 F-14_03.jpg|280px]] | |||
|[[Image:W06 MLA1 nLOF D220 F-7_03.jpg|280px]] | |||
|[[Image:W06 MLA1 nLOF D220 F-4_2_03.jpg|280px]] | |||
|[[Image:W06 MLA1 nLOF D220 F-1_03.jpg|280px]] | |||
|[[Image:W06 MLA1 nLOF D220 F6_03.jpg|280px]] | |||
|} | |||
<br clear="all" /> | |||
'''SEM images of 2µm AZ nLOF 2020 as a function of defocus parameter for Aligner: Maskless 02 (MLA2) using dose 450mJ/cm<sup>2</sup>:''' | |||
{|border="1" cellspacing="0" cellpadding="3" style="text-align:left;" | |||
|- | |||
|- | |||
|-style="background:silver; color:black" | |||
! | |||
!Defoc 0 | |||
!Defoc 2 | |||
!Defoc 4 | |||
|- | |||
|- | |||
|-style="background:WhiteSmoke; color:black" | |||
|2µm triplets | |||
|[[Image:W17 mla2 nLOF D450 F0_04.jpg|340px]] | |||
|[[Image:W17 mla2 nLOF D450 F2_01.jpg|340px]] | |||
|[[Image:W17 mla2 nLOF D450 F4_02.jpg|340px]] | |||
|- | |||
|-style="background:WhiteSmoke; color:black" | |||
|Lines | |||
|[[Image:W17 mla2 nLOF D450 F0_03.jpg|340px]] | |||
|[[Image:W17 mla2 nLOF D450 F2_02.jpg|340px]] | |||
|[[Image:W17 mla2 nLOF D450 F4_03.jpg|340px]] | |||
|} | |} | ||
<br clear="all" /> | <br clear="all" /> | ||
Latest revision as of 14:55, 10 September 2026
The content on this page, including all images and pictures, was created by DTU Nanolab staff, unless otherwise stated.
Feedback to this page: click here
Mask Aligner vs Maskless Aligner
In the first half of 2026, a rather thorough investigation of the differences between exposure using mask aligner and maskless aligner was conducted. The result was presented as an advanced lithography tutorial at the 2026 Nordic Nanolab User Meeting in Uppsala, Sweden.
Slides presented at NNUM in Uppsala: MA6 vs MLA 2026_v09
Mask design used in the investigation: LithoTestAlign_2025_v10.gds
Tools used in the investigation
- Wafers
- 100mm Si, SSP <100>
- Resists
- AZ 5214E (image reversal resist, but processed positive)
- AZ MiR 701 (positive tone resist)
- AZ nLOF 2020 (negative tone resist)
- Spin coating (incl. HMDS)
- Exposure
- Aligner: MA6-2
- Aligner: MA6-1 (in PolyFabLab)
- Aligner: Maskless 02
- Aligner: Maskless 01
- Development (incl. PEB, if relevant)
- Inspection
Data from the investigation
AZ 5214E
Resolution (AZ 5214E)
Resolution at optimal processing conditions for 1.5µm AZ 5214E using different exposure equipment:
| Exposure equipment | Dose [mJ/cm2] | Contact/Defoc | Resolution [µm] | Comment |
|---|---|---|---|---|
| Aligner: MA6-2 | 100 | Vacuum | 1 | |
| Aligner: MA6-1 | 100 | Vacuum | 1.25 | Probably over-exposed |
| Aligner: Maskless 02 (MLA2) | 90 | 2 | 1.25 |
SEM images from different exposure equipment for 1.5µm AZ 5214E at optimal processing conditions:
| 2µm triplets | Lines | Trenches | |
|---|---|---|---|
| Aligner: MA6-2
100mJ/cm2, vacuum contact |
|||
| Aligner: MA6-1
100mJ/cm2, vacuum contact |
|||
| Aligner: Maskless 02 (MLA2)
90mJ/cm2, defoc 2 |
SEM images of different size structures for 1.5µm AZ 5214E:
| 1µm triplets | 2µm triplets | 4µm triplets | |
|---|---|---|---|
| Aligner: MA6-1
100mJ/cm2, vacuum contact |
Yield (AZ 5214E)
The yield is measured by inspecting all 116 lithographic resolution test structures in an optical microscope and recording the smallest resolved dots and lines.
Effect of exposure mode for mask aligner
Effect of WEC pressure for mask aligner (after WEC head service)
Resist profile (AZ 5214E)
Linewidth and sidewall angle vs exposure dose (AZ 5214E)
Result of image analysis of SEM images of 2µm triplets:
SEM images of 1.5µm AZ 5214E as a function of exposure dose for Aligner: MA6-2 using vacuum contact:
| 85mJ/cm2 | 90mJ/cm2 | 95mJ/cm2 | 100mJ/cm2 | 105mJ/cm2 | |
|---|---|---|---|---|---|
| 2µm triplets | |||||
| Lines |
SEM images of 1.5µm AZ 5214E as a function of exposure dose for Aligner: Maskless 02 (MLA2) using defoc 2:
| 80mJ/cm2 | 90mJ/cm2 | 100mJ/cm2 | 110mJ/cm2 | |
|---|---|---|---|---|
| 2µm triplets | ||||
| Trenches and Lines |
Linewidth and sidewall angle vs defocus parameter (AZ 5214E)
Result of image analysis of SEM images of 2µm triplets:
| Linewidth and sidewall angle vs. defocus value for 1.5µm AZ 5214E exposed in Aligner: Maskless 02 (MLA2) using dose 95mJ/cm2. Blue circles: Width of 2µm line. Orange Squares: Sidewall angle. |
SEM images of 1.5µm AZ 5214E as a function of defocus parameter for Aligner: Maskless 02 (MLA2) using dose 95mJ/cm2:
| Defoc -8 | Defoc -1 | Defoc 2 | Defoc 5 | Defoc 12 | |
|---|---|---|---|---|---|
| 2µm triplets | |||||
| Lines |
AZ MiR 701
Resolution (AZ MiR 701)
Resolution at optimal processing conditions for 1.5µm AZ MiR 701 using different exposure equipment:
| Exposure equipment | Dose [mJ/cm2] | Contact/Defoc | Resolution [µm] | Comment |
|---|---|---|---|---|
| Aligner: MA6-2 | 220 | Vacuum | 1 | |
| Aligner: Maskless 02 (MLA2) | 275 | 2 | 1 |
SEM images of 1.5µm AZ MiR 701 from different exposure equipment at optimal processing conditions:
| 2µm triplets | Lines | Trenches | |
|---|---|---|---|
| Aligner: MA6-2
220mJ/cm2, vacuum contact |
|||
| Aligner: Maskless 02 (MLA2)
275mJ/cm2, defoc 2 |
Resist profile (AZ MiR 701)
Linewidth and sidewall angle vs exposure dose (AZ MiR 701)
Result of image analysis of SEM images of 2µm triplets:
SEM images of 1.5µm AZ MiR 701 as a function of exposure dose for Aligner: MA6-2 using vacuum contact:
| 160mJ/cm2 | 190mJ/cm2 | 220mJ/cm2 | 250mJ/cm2 | 280mJ/cm2 | |
|---|---|---|---|---|---|
| 2µm triplets | |||||
| Lines |
SEM images of 1.5µm AZ MiR 701 as a function of exposure dose for Aligner: Maskless 02 (MLA2) using defoc 2:
| 225mJ/cm2 | 275mJ/cm2 | 325mJ/cm2 | 375mJ/cm2 | |
|---|---|---|---|---|
| 2µm triplets | ||||
| Lines |
Linewidth and sidewall angle vs defocus parameter (AZ MiR 701)
Result of image analysis of SEM images of 2µm triplets:
| Linewidth and sidewall angle vs. defocus value for 1.5µm AZ MiR 701 exposed in Aligner: Maskless 02 (MLA2) using dose 95mJ/cm2. Blue circles: Width of 2µm line. Orange Squares: Sidewall angle. |
SEM images of 1.5µm AZ MiR 701 as a function of defocus parameter for Aligner: Maskless 02 (MLA2) using dose 275mJ/cm2:
| Defoc -1 | Defoc 1 | Defoc 2 | Defoc 3 | Defoc 5 | |
|---|---|---|---|---|---|
| 2µm triplets | |||||
| Lines |
AZ nLOF 2020
Resolution (AZ nLOF 2020)
Resolution at optimal processing conditions for 2µm AZ nLOF 2020 using different exposure equipment:
| Exposure equipment | Dose [mJ/cm2] | Contact/Defoc | Resolution [µm] | Comment |
|---|---|---|---|---|
| Aligner: MA6-2 | 154 | Vacuum | 1 | |
| Aligner: Maskless 01 (MLA1) | 220 | -4 | 2 | |
| Aligner: Maskless 02 (MLA2) | 450 | 0 | 1.25 |
SEM images of 2µm AZ nLOF 2020 from different exposure equipment at optimal processing conditions:
| 2µm triplets | Lines | Trenches | |
|---|---|---|---|
| Aligner: MA6-2
154mJ/cm2, vacuum contact |
|||
| Aligner: Maskless 01 (MLA1)
220mJ/cm2, Defoc -4 |
|||
| Aligner: Maskless 02 (MLA2)
450mJ/cm2, defoc 0 |
SEM images of different size structures for 2µm AZ nLOF 2020:
| 1µm triplets | 2µm triplets | 4µm triplets | |
|---|---|---|---|
| Aligner: MA6-2
154mJ/cm2, vacuum contact |
|||
| Aligner: Maskless 01 (MLA1)
220mJ/cm2, Defoc -4 |
Cross-sectional SEM images of 2µm AZ nLOF 2020 at optimal processing conditions:
| 2µm lines | 2µm trenches | Lines | Trenches | |
|---|---|---|---|---|
| Aligner: Maskless 01 (MLA1)
220mJ/cm2, Defoc -4 |
Resist profile (AZ nLOF 2020)
Linewidth and sidewall angle vs exposure dose (AZ nLOF 2020)
Result of image analysis of SEM images of 2µm triplets:
SEM images of 2µm AZ nLOF 2020 as a function of exposure dose for Aligner: MA6-2 using vacuum contact:
| 100mJ/cm2 | 120mJ/cm2 | 140mJ/cm2 | 160mJ/cm2 | |
|---|---|---|---|---|
| 2µm triplets |
SEM images of 2µm AZ nLOF 2020 as a function of exposure dose for Aligner: Maskless 01 (MLA1) using defoc -4:
| 200mJ/cm2 | 220mJ/cm2 | 240mJ/cm2 | |
|---|---|---|---|
| 2µm triplets |
SEM images of 2µm AZ nLOF 2020 as a function of exposure dose for Aligner: Maskless 02 (MLA2) using defoc 0:
| 400mJ/cm2 | 450mJ/cm2 | 500mJ/cm2 | |
|---|---|---|---|
| 2µm triplets |
Linewidth and sidewall angle vs defocus parameter (AZ nLOF 2020)
Result of image analysis of SEM images of 2µm triplets:
SEM images of 2µm AZ nLOF 2020 as a function of defocus parameter for Aligner: Maskless 01 (MLA1) using dose 220mJ/cm2:
| Defoc -14 | Defoc -7 | Defoc -4 | Defoc -1 | Defoc -6 | |
|---|---|---|---|---|---|
| 2µm triplets | |||||
| Lines |
SEM images of 2µm AZ nLOF 2020 as a function of defocus parameter for Aligner: Maskless 02 (MLA2) using dose 450mJ/cm2:
| Defoc 0 | Defoc 2 | Defoc 4 | |
|---|---|---|---|
| 2µm triplets | |||
| Lines |