'''Feedback to this page''': '''[mailto:labadviser@nanolab.dtu.dk?Subject=Feed%20back%20from%20page%20http://labadviser.nanolab.dtu.dk/index.php?title=Specific_Process_Knowledge/Lithography/Aligners/MAvsMLA click here]'''
'''Feedback to this page''': '''[mailto:taran@nanolab.dtu.dk?Subject=Feed%20back%20from%20page%20http://labadviser.nanolab.dtu.dk/index.php?title=Specific_Process_Knowledge/Lithography/Aligners/MAvsMLA click here]'''


[[Category: Equipment|Lithography exposure]]
[[Category:Equipment|Lithography exposure]]
[[Category: Lithography|Exposure]]
[[Category:Lithography|Exposure]]


__TOC__
__TOC__
Line 10: Line 10:
=Mask Aligner vs Maskless Aligner=
=Mask Aligner vs Maskless Aligner=


Slides presented at NNUM in Uppsala 2026: [[media:MA6 vs MLA 2026_v09.pdf|'''MA6 vs MLA 2026_v09''']]
In the first half of 2026, a rather thorough investigation of the differences between exposure using mask aligner and maskless aligner was conducted. The result was presented as an advanced lithography tutorial at the 2026 Nordic Nanolab User Meeting in Uppsala, Sweden.


Mask design used in the investigation: [[media:LithoTestAlign_2025_v10.gds|LithoTestAlign_2025_v10.gds]]
Slides presented at NNUM in Uppsala: [[Media:MA6 vs MLA 2026 v09.pdf|'''MA6 vs MLA 2026_v09''']]


=Additional data=
Mask design used in the investigation: [[Media:LithoTestAlign 2025 v10.gds|LithoTestAlign_2025_v10.gds]]
<span style="background:#FF2800">THIS PAGE IS UNDER CONSTRUCTION</span>[[image:Under_construction.png|200px]]
<br clear="all" />


==AZ 5214E==
=Tools used in the investigation=
===Resolution===
*Wafers
* Table with optimal parameters and resolution for different aligners
**100mm Si, SSP <100>
* SEM pictures
*Resists
**[[Specific_Process_Knowledge/Lithography/5214E|AZ 5214E]] (image reversal resist, but processed positive)
**[[Specific_Process_Knowledge/Lithography/MiR|AZ MiR 701]] (positive tone resist)
**[[Specific_Process_Knowledge/Lithography/nLOF|AZ nLOF 2020]] (negative tone resist)
*Spin coating (incl. HMDS)
**[[Specific_Process_Knowledge/Lithography/Coaters#Spin_Coater:_Gamma_UV|Spin Coater: Gamma UV]]
*Exposure
**[[Specific_Process_Knowledge/Lithography/UVExposure/aligner_MA6-2|Aligner: MA6-2]]
**[[Specific_Process_Knowledge/Lithography/UVExposure/aligner_MA6-1|Aligner: MA6-1]] (in PolyFabLab)
**[[Specific Process Knowledge/Lithography/UVExposure/aligner_MLA2|Aligner: Maskless 02]]
**[[Specific Process Knowledge/Lithography/UVExposure/aligner_MLA1|Aligner: Maskless 01]]
*Development (incl. PEB, if relevant)
**[[Specific_Process_Knowledge/Lithography/Development/UV_developer|Developer: TMAH UV-lithography]]
*Inspection
**[[Specific_Process_Knowledge/Characterization/Optical_microscope|Microscope Olympus MX63]]
**[[Specific_Process_Knowledge/Characterization/SEM_Supra_1|SEM Supra 1]]
**[[Specific_Process_Knowledge/Characterization/SEM_Supra_3|SEM Supra 3]]
<br clear="all" />
<br clear="all" />


===Yield===
=Data from the investigation=
* Wafer maps of:
<!-- <span style="background:#FF2800">THIS PAGE IS UNDER CONSTRUCTION</span>[[image:Under_construction.png|200px]]
** Aligner: Maskless 02 (MLA2)
-->
** Aligner: MA6-1
<br clear="all" />
** Aligner: MA6-2 before service
==AZ 5214E==
** Aligner: MA6-2 after service + WEC pressure
<br clear="all" />
===Resolution (AZ 5214E)===
<br clear="all" />
'''Resolution at optimal processing conditions for 1.5µm AZ 5214E using different exposure equipment:'''
{| class="wikitable"
|+
!Exposure equipment
!Dose [mJ/cm<sup>2</sup>]
!Contact/Defoc
!Resolution [µm]
!Comment
|-
|Aligner: MA6-2
|100
|Vacuum
|1
|
|-
|Aligner: MA6-1
|100
|Vacuum
|1.25
|Probably over-exposed
|-
|Aligner: Maskless 02 (MLA2)
|90
|2
|1.25
|
|}
<br clear="all" />
 
'''SEM images from different exposure equipment for 1.5µm AZ 5214E at optimal processing conditions:'''
 
{|border="1" cellspacing="0" cellpadding="3" style="text-align:left;"
|-
 
|-
|-style="background:silver; color:black"
!
!2µm triplets
!Lines
!Trenches
|-
 
|-
|-style="background:WhiteSmoke; color:black"
|Aligner: MA6-2
100mJ/cm<sup>2</sup>, vacuum contact
|[[Image:W14 MA62 5214E vac D100_B4T_01.jpg|400px]]
|[[Image:W14 MA62 5214E vac D100_B4T_02.jpg|400px]]
|[[Image:W14 MA62 5214E vac D100_B4T_03.jpg|400px]]
 
|-
|-style="background:WhiteSmoke; color:black"
|Aligner: MA6-1
100mJ/cm<sup>2</sup>, vacuum contact <br>(probably over-exposed)
|[[Image:W32 PFL 5214 D100 vac C6B_01.jpg|400px]]
|[[Image:W32 PFL 5214 D100 vac C6B_04.jpg|400px]]
|[[Image:W32 PFL 5214 D100 vac C6B_05.jpg|400px]]
 
|-
|-style="background:WhiteSmoke; color:black"
|Aligner: Maskless 02 (MLA2)
90mJ/cm<sup>2</sup>, defoc 2
|[[Image:W13 mla2 5214E D90 F2_05.jpg|400px]]
|[[Image:W13 mla2 5214E D90 F2_01.jpg|400px]]
|[[Image:W13 mla2 5214E D90 F2_02.jpg|400px]]
 
|}
<br clear="all" />
 
'''SEM images of different size structures for 1.5µm AZ 5214E:'''
 
{|border="1" cellspacing="0" cellpadding="3" style="text-align:left;"
|-
 
|-
|-style="background:silver; color:black"
!
!1µm triplets
!2µm triplets
!4µm triplets
|-
 
|-
|-style="background:WhiteSmoke; color:black"
|Aligner: MA6-1
100mJ/cm<sup>2</sup>, vacuum contact <br>(probably over-exposed)
|[[Image:W32 PFL 5214 D100 vac C6B_02.jpg|400px]]
|[[Image:W32 PFL 5214 D100 vac C6B_01.jpg|400px]]
|[[Image:W32 PFL 5214 D100 vac C6B_03.jpg|400px]]
 
|}
<br clear="all" />
 
===Yield (AZ 5214E)===
 
The yield is measured by inspecting all 116 lithographic resolution test structures in an optical microscope and recording the smallest resolved dots and lines.
<br clear="all" />
<br clear="all" />


{| cellpadding="2" style="border: 2px solid darkgray;" align="center"
{| cellpadding="2" style="border: 2px solid darkgray;" align="center"
! width="320" |  
! width="460" |  
! width="320" |  
! width="460" |  
! width="320" |  
! width="460" |  


|+'''Wafer maps at optimal processing conditions for different aligners'''
|+'''Wafer maps for 1.5µm AZ 5214E at optimal processing conditions for different aligners'''
|- border="0" align="center"
|- border="0" align="center"
|[[Map_MLA2_D90_F2.jpg|300px]]
|[[Image:Map_MLA2_D90_F2.jpg|450px]]
|[[Map_MA6-2_vacuum.jpg|300px]]
|[[Image:Map_MA6-2_vacuum.jpg|450px]]
|[[Map_MA6-1_vacuum.jpg|300px]]
|[[Image:Map_MA6-1_vacuum.jpg|450px]]


|- align="center"
|- align="center"
| Aligner: MAskless 02 (MLA2). ||  Aligner: MA6-2 || Aligner: MA6-1
| Aligner: Maskless 02 (MLA2) (Dose 90mJ/cm<sup>2</sup>; defoc 2). <br/>Resolution: 1.22µm average; 0.1µm standard deviation. <br/>Yield at 1.25µm: 99% ||  Aligner: MA6-2 (Dose 100mJ/cm<sup>2</sup>; vacuum contact). <br/>Resolution: 1.02µm average; 0.1µm standard deviation. <br/>Yield at 1.25µm: 100% || Aligner: MA6-1 (Dose 100mJ/cm<sup>2</sup>; vacuum contact). Probably over-exposed. <br/>Resolution: 1.30µm average; 0.2µm standard deviation. <br/>Yield at 1.25µm: 59%
|}
<br clear="all" />
 
====Effect of exposure mode for mask aligner====
{| cellpadding="2" style="border: 2px solid darkgray;" align="center"
! width="460" |
! width="460" |
! width="460" |
 
|+'''Wafer maps for 1.5µm AZ 5214E at different exposure modes for Aligner: MA6-2 (Dose 100mJ/cm<sup>2</sup>)'''
|- border="0" align="center"
|[[Image:Map_MA6-2_hard.jpg|450px]]
|[[Image:Map_MA6-2_soft_clean.jpg|450px]]
|[[Image:Map_MA6-2_prox.jpg|450px]]


|- align="center"
| Hard contact. <br/>Resolution: 1.17µm average; 0.2µm standard deviation. <br/>Yield at 1.25µm: 89% || Soft contact. <br/>Resolution: 3.77µm average; 0.7µm standard deviation. <br/>Yield at 2.5µm: 4% || 10µm proximity. <br/>Resolution: 4.19µm average; 0.7µm standard deviation. <br/>Yield at 2.5µm: 3%
|}
|}
<br clear="all" />
<br clear="all" />


===Resist profile (sidewall angle and linewidth)===
{| cellpadding="2" style="border: 2px solid darkgray;" align="center"
*SEM pictures to support graphs?
! width="460" |
! width="460" |
! width="460" |


[[Image:5214E_Linewidth vs dose.jpg|left|500px|thumb|Width of 2µm line vs. exposure dose for 1.5µm AZ 5214E. <br>Blue circles: Exposed on Aligner: MA6-2 in vacuum contact. <br>Orange Squares: Exposed on Aligner: Maskless 02 (MLA2) using defoc 2 (QC defoc=2).]]
|+'''Wafer maps for 1.5µm AZ 5214E at different exposure modes for Aligner: MA6-1 (Dose 100mJ/cm<sup>2</sup>, probably over-exposed)'''
|- border="0" align="center"
|[[Image:Map_MA6-1_hard.jpg|450px]]
|[[Image:Map_MA6-1_soft.jpg|450px]]
|[[Image:Map_MA6-1_prox.jpg|450px]]


[[Image:5214E_Sidewall vs dose.jpg|left|500px|thumb|Sidewall angle vs. exposure dose for 1.5µm AZ 5214E. <br>Blue circles: Exposed on Aligner: MA6-2 in vacuum contact. <br>Orange Squares: Exposed on Aligner: Maskless 02 (MLA2) using defoc 2 (QC defoc=2).]]
|- align="center"
| Hard contact. <br/>Resolution: 1.58µm average; 0.5µm standard deviation. <br/>Yield at 1.25µm: 48% || Soft contact. <br/>Resolution: 2.36µm average; 0.4µm standard deviation. <br/>Yield at 2.5µm: 80% <br/>At dose 92mJ/cm<sup>2</sup>, the average resolution decreases to 1.91µm and the yield at 2.5µm increases to 100% || 10µm proximity. <br/>Resolution: 2.73µm average; 0.6µm standard deviation. <br/>Yield at 2.5µm: 53%
|}
<br clear="all" />


[[Image:5214E_Profile vs defoc.jpg|left|500px|thumb|Linewidth and sidewall angle vs. defocus value  for 1.5µm AZ 5214E exposed in Aligner: Maskless 02 (MLA2) using dose 95mJ/cm<sup>2</sup>. <br>Blue circles: Width of 2µm line. Orange Squares: Sidewall angle.]]
====Effect of WEC pressure for mask aligner (after WEC head service)====
<!--
{| cellpadding="2" style="border: 2px solid darkgray;" align="center"
{| cellpadding="2" style="border: 2px solid darkgray;" align="center"
! width="350" |  
! width="460" |  
! width="350" |  
! width="460" |


|+'''Lithographic result vs. exposure dose. Data by Thomas Anhøj @ DTU Nanolab, 2026.'''
|+'''Wafer maps for 1.5µm AZ 5214E at different WEC pressure for Aligner: MA6-2 (Dose 100mJ/cm<sup>2</sup>)'''
|- border="0" align="center"
|- border="0" align="center"
|[[Image:5214E_Linewidth vs dose.jpg|450px]]
|[[Image:Map_MA6-2_soft_WEC015.jpg|450px]]
|[[Image:5214E_Sidewall vs dose.jpg|450px]]
|[[Image:Map_MA6-2_soft_WEC040.jpg|450px]]


|- align="center"
|- align="center"
| Width of 2µm line vs. exposure dose. <br>Blue circles: Exposed on Aligner: MA6-2 in vacuum contact. <br>Orange Squares: Exposed on Aligner: Maskless 02 (MLA2) using defoc 2 (QC defoc=2). || Sidewall angle vs. exposure dose. <br>Blue circles: Exposed on Aligner: MA6-2 in vacuum contact. <br>Orange Squares: Exposed on Aligner: Maskless 02 (MLA2) using defoc 2 (QC defoc=2).
| Soft contact, 0.15bar WEC pressure. <br/>Resolution: 3.92µm average; 0.9µm standard deviation. <br/>Yield at 2.5µm: 8% || Soft contact, 0.40bar WEC pressure. <br/>Resolution: 2.19µm average; 0.5µm standard deviation. <br/>Yield at 2.5µm: 86%
 
|- border="0" align="center"
|[[Image:Map_MA6-2_prox_WEC015.jpg|450px]]
|[[Image:Map_MA6-2_prox_WEC040.jpg|450px]]
 
|- align="center"
| 10µm proximity, 0.15bar WEC pressure. <br/>Resolution: 3.22µm average; 0.8µm standard deviation. <br/>Yield at 2.5µm: 34% || 10µm proximity, 0.40bar WEC pressure. <br/>Resolution: 2.83µm average; 0.6µm standard deviation. <br/>Yield at 2.5µm: 66%
|}
<br clear="all" />
 
===Resist profile (AZ 5214E)===
<br clear="all" />
====Linewidth and sidewall angle vs exposure dose (AZ 5214E)====
<br clear="all" />
'''Result of image analysis of SEM images of 2µm triplets:'''
 
{| cellpadding="2" style="border: 2px solid darkgray;" align="left"
! width="510" | 
 
|+
|- border="0" align="center"
|[[Image:5214E_Linewidth vs dose.jpg|500px]]
|[[Image:5214E_Sidewall vs dose.jpg|500px]]
 
|- align="center"
| colspan="2" | Width of 2µm line and sidewall angle vs. exposure dose for 1.5µm AZ 5214E. <br>Blue circles: Exposed on Aligner: MA6-2 in vacuum contact. <br>Orange Squares: Exposed on Aligner: Maskless 02 (MLA2) using defoc 2 (QC defoc=2).
|}
<br clear="all" />
 
 
'''SEM images of 1.5µm AZ 5214E as a function of exposure dose for Aligner: MA6-2 using vacuum contact:'''
 
{|border="1" cellspacing="0" cellpadding="3" style="text-align:left;"
|-
 
|-
|-style="background:silver; color:black"
!
!85mJ/cm<sup>2</sup>
!90mJ/cm<sup>2</sup>
!95mJ/cm<sup>2</sup>
!100mJ/cm<sup>2</sup>
!105mJ/cm<sup>2</sup>
|-
 
|-
|-style="background:WhiteSmoke; color:black"
|2µm triplets
|[[Image:W14 MA62 5214E vac D85_H6B_01.jpg|280px]]
|[[Image:W14 MA62 5214E vac D90_H4B_01.jpg|280px]]
|[[Image:W14 MA62 5214E vac D95_F3B_01.jpg|280px]]
|[[Image:W14 MA62 5214E vac D100_B4T_01.jpg|280px]]
|[[Image:W14 MA62 5214E vac D105_C6T_01.jpg|280px]]
 
|-
|-style="background:WhiteSmoke; color:black"
|Lines
|[[Image:W14 MA62 5214E vac D85_H6B_02.jpg|280px]]
|[[Image:W14 MA62 5214E vac D90_H4B_02.jpg|280px]]
|[[Image:W14 MA62 5214E vac D95_F3B_02.jpg|280px]]
|[[Image:W14 MA62 5214E vac D100_B4T_02.jpg|280px]]
|[[Image:W14 MA62 5214E vac D105_C6T_02.jpg|280px]]
 
|}
<br clear="all" />
 
'''SEM images of 1.5µm AZ 5214E as a function of exposure dose for Aligner: Maskless 02 (MLA2) using defoc 2:'''
 
{|border="1" cellspacing="0" cellpadding="3" style="text-align:left;"
|-
 
|-
|-style="background:silver; color:black"
!
!80mJ/cm<sup>2</sup>
!90mJ/cm<sup>2</sup>
!100mJ/cm<sup>2</sup>
!110mJ/cm<sup>2</sup>
|-
 
|-
|-style="background:WhiteSmoke; color:black"
|2µm triplets
|[[Image:W13 mla2 5214E D80 F2_02.jpg|280px]]
|[[Image:W13 mla2 5214E D90 F2_05.jpg|280px]]
|[[Image:W13 mla2 5214E D100 F2_01.jpg|280px]]
|[[Image:W13 mla2 5214E D110 F2_01.jpg|280px]]
 
|-
|-style="background:WhiteSmoke; color:black"
|Trenches <br>and Lines
|[[Image:W13 mla2 5214E D80 F2_01.jpg|280px]]
|[[Image:W13 mla2 5214E D90 F2_04.jpg|280px]]
|[[Image:W13 mla2 5214E D100 F2_02.jpg|280px]]
|[[Image:W13 mla2 5214E D110 F2_02.jpg|280px]]
 
|}
<br clear="all" />
 
====Linewidth and sidewall angle vs defocus parameter (AZ 5214E)====
<br clear="all" />
'''Result of image analysis of SEM images of 2µm triplets:'''
 
{| cellpadding="2" style="border: 2px solid darkgray;" align="left"
! width="510" |
 
|+
|- border="0" align="center"
|[[Image:5214E_Profile vs defoc.jpg|500px]]
 
|- align="center"
| Linewidth and sidewall angle vs. defocus value  for 1.5µm AZ 5214E exposed in Aligner: Maskless 02 (MLA2) using dose 95mJ/cm<sup>2</sup>. <br>Blue circles: Width of 2µm line. <br>Orange Squares: Sidewall angle.
 
|}
<br clear="all" />
 
 
'''SEM images of 1.5µm AZ 5214E as a function of defocus parameter for Aligner: Maskless 02 (MLA2) using dose 95mJ/cm<sup>2</sup>:'''
 
{|border="1" cellspacing="0" cellpadding="3" style="text-align:left;"
|-
 
|-
|-style="background:silver; color:black"
!
!Defoc -8
!Defoc -1
!Defoc 2
!Defoc 5
!Defoc 12
|-
 
|-
|-style="background:WhiteSmoke; color:black"
|2µm triplets
|[[Image:W33 MLA2 5214 F-8 D95_101.jpg|280px]]
|[[Image:W33 MLA2 5214 F-1 D95_01.jpg|280px]]
|[[Image:W33 MLA2 5214 F2 D95_01.jpg|280px]]
|[[Image:W33 MLA2 5214 F5 D95_01.jpg|280px]]
|[[Image:W33 MLA2 5214 F12 D95_101.jpg|280px]]
 
|-
|-style="background:WhiteSmoke; color:black"
|Lines
|[[Image:W33 MLA2 5214 F-8 D95_102.jpg|280px]]
|[[Image:W33 MLA2 5214 F-1 D95_02.jpg|280px]]
|[[Image:W33 MLA2 5214 F2 D95_1_02.jpg|280px]]
|[[Image:W33 MLA2 5214 F5 D95_02.jpg|280px]]
|[[Image:W33 MLA2 5214 F12 D95_102.jpg|280px]]


|}
|}
-->
<br clear="all" />
<br clear="all" />


==AZ MiR 701==
==AZ MiR 701==
===Resolution===
<br clear="all" />
* Table with optimal parameters and resolution for different aligners
===Resolution (AZ MiR 701)===
* SEM pictures
<br clear="all" />
'''Resolution at optimal processing conditions for 1.5µm AZ MiR 701 using different exposure equipment:'''
{| class="wikitable"
|+
!Exposure equipment
!Dose [mJ/cm<sup>2</sup>]
!Contact/Defoc
!Resolution [µm]
!Comment
|-
|Aligner: MA6-2
|220
|Vacuum
|1
|
|-
|Aligner: Maskless 02 (MLA2)
|275
|2
|1
|
|}
<br clear="all" />
 
'''SEM images of 1.5µm AZ MiR 701 from different exposure equipment at optimal processing conditions:'''
 
{|border="1" cellspacing="0" cellpadding="3" style="text-align:left;"
|-
 
|-
|-style="background:silver; color:black"
!
!2µm triplets
!Lines
!Trenches
|-
 
|-
|-style="background:WhiteSmoke; color:black"
|Aligner: MA6-2
220mJ/cm<sup>2</sup>, vacuum contact
|[[Image:W18 MA62 MiR vac D220_I3T_03.jpg|400px]]
|[[Image:W18 MA62 MiR vac D220_I3T_02.jpg|400px]]
|[[Image:W18 MA62 MiR vac D220_I3T_01.jpg|400px]]
 
|-
|-style="background:WhiteSmoke; color:black"
|Aligner: Maskless 02 (MLA2)
275mJ/cm<sup>2</sup>, defoc 2
|[[Image:W15 MLA2 MiR F2 D275_03.jpg|400px]]
|[[Image:W15 MLA2 MiR F2 D275_02.jpg|400px]]
|[[Image:W15 MLA2 MiR F2 D275_01.jpg|400px]]
 
|}
<br clear="all" />
 
===Resist profile (AZ MiR 701)===
<br clear="all" />
 
====Linewidth and sidewall angle vs exposure dose (AZ MiR 701)====
<br clear="all" />
 
'''Result of image analysis of SEM images of 2µm triplets:'''
 
{| cellpadding="2" style="border: 2px solid darkgray;" align="left"
! width="510" | 
 
|+
|- border="0" align="center"
|[[Image:MiR_Linewidth vs dose.jpg|500px]]
|[[Image:MiR_Sidewall vs dose.jpg|500px]]
 
|- align="center"
| colspan="2" | Width of 2µm line and sidewall angle vs. exposure dose for 1.5µm AZ MiR 701. <br>Blue circles: Exposed on Aligner: MA6-2 in vacuum contact. <br>Orange Squares: Exposed on Aligner: Maskless 02 (MLA2) using defoc 2 (QC defoc=2). 
|}
<br clear="all" />
 
 
'''SEM images of 1.5µm AZ MiR 701 as a function of exposure dose for Aligner: MA6-2 using vacuum contact:'''
{|border="1" cellspacing="0" cellpadding="3" style="text-align:left;"
|-
 
|-
|-style="background:silver; color:black"
!
!160mJ/cm<sup>2</sup>
!190mJ/cm<sup>2</sup>
!220mJ/cm<sup>2</sup>
!250mJ/cm<sup>2</sup>
!280mJ/cm<sup>2</sup>
|-
 
|-
|-style="background:WhiteSmoke; color:black"
|2µm triplets
|[[Image:W18 MA62 MiR vac D160_F8T_04.jpg|280px]]
|[[Image:W18 MA62 MiR vac D190_H6B_03.jpg|280px]]
|[[Image:W18 MA62 MiR vac D220_I3T_03.jpg|280px]]
|[[Image:W18 MA62 MiR vac D250_F3T_03.jpg|280px]]
|[[Image:W18 MA62 MiR vac D280_D5B_03.jpg|280px]]
 
|-
|-style="background:WhiteSmoke; color:black"
|Lines
|[[Image:W18 MA62 MiR vac D160_F8T_02.jpg|280px]]
|[[Image:W18 MA62 MiR vac D190_H6B_02.jpg|280px]]
|[[Image:W18 MA62 MiR vac D220_I3T_02.jpg|280px]]
|[[Image:W18 MA62 MiR vac D250_F3T_02.jpg|280px]]
|[[Image:W18 MA62 MiR vac D280_D5B_02.jpg|280px]]
 
|}
<br clear="all" />
 
'''SEM images of 1.5µm AZ MiR 701 as a function of exposure dose for Aligner: Maskless 02 (MLA2) using defoc 2:'''
{|border="1" cellspacing="0" cellpadding="3" style="text-align:left;"
|-
 
|-
|-style="background:silver; color:black"
!
!225mJ/cm<sup>2</sup>
!275mJ/cm<sup>2</sup>
!325mJ/cm<sup>2</sup>
!375mJ/cm<sup>2</sup>
|-
 
|-
|-style="background:WhiteSmoke; color:black"
|2µm triplets
|[[Image:W15 MLA2 MiR F2 D225_04.jpg|280px]]
|[[Image:W15 MLA2 MiR F2 D275_03.jpg|280px]]
|[[Image:W15 MLA2 MiR F2 D325_03.jpg|280px]]
|[[Image:W15 MLA2 MiR F2 D375_03.jpg|280px]]
 
|-
|-style="background:WhiteSmoke; color:black"
|Lines
|[[Image:W15 MLA2 MiR F2 D225_01.jpg|280px]]
|[[Image:W15 MLA2 MiR F2 D275_02.jpg|280px]]
|[[Image:W15 MLA2 MiR F2 D325_01.jpg|280px]]
|[[Image:W15 MLA2 MiR F2 D375_01.jpg|280px]]
 
|}
<br clear="all" />
 
====Linewidth and sidewall angle vs defocus parameter (AZ MiR 701)====
<br clear="all" />
 
'''Result of image analysis of SEM images of 2µm triplets:'''
{| cellpadding="2" style="border: 2px solid darkgray;" align="left"
! width="510" |
 
|+
|- border="0" align="center"
|[[Image:MiR_Profile vs defoc.jpg|500px]]
 
|- align="center"
| Linewidth and sidewall angle vs. defocus value  for 1.5µm AZ MiR 701 exposed in Aligner: Maskless 02 (MLA2) using dose 95mJ/cm<sup>2</sup>. <br>Blue circles: Width of 2µm line. <br>Orange Squares: Sidewall angle.
 
|}
<br clear="all" />
 


===Resist profile (sidewall angle and linewidth)===
'''SEM images of 1.5µm AZ MiR 701 as a function of defocus parameter for Aligner: Maskless 02 (MLA2) using dose 275mJ/cm<sup>2</sup>:'''
*SEM pictures to support graphs?
{|border="1" cellspacing="0" cellpadding="3" style="text-align:left;"
|-


[[Image:MiR_Linewidth vs dose.jpg|left|500px|thumb|Width of 2µm line vs. exposure dose for 1.5µm AZ MiR 701. <br>Blue circles: Exposed on Aligner: MA6-2 in vacuum contact. <br>Orange Squares: Exposed on Aligner: Maskless 02 (MLA2) using defoc 2 (QC defoc=2).]]
|-
|-style="background:silver; color:black"
!
!Defoc -1
!Defoc 1
!Defoc 2
!Defoc 3
!Defoc 5
|-


[[Image:MiR_Sidewall vs dose.jpg|left|500px|thumb|Sidewall angle vs. exposure dose for 1.5µm AZ MiR 701. <br>Blue circles: Exposed on Aligner: MA6-2 in vacuum contact. <br>Orange Squares: Exposed on Aligner: Maskless 02 (MLA2) using defoc 2 (QC defoc=2).]]
|-
|-style="background:WhiteSmoke; color:black"
|2µm triplets
|[[Image:W15 MLA2 MiR F-1 D275_01.jpg|280px]]
|[[Image:W15 MLA2 MiR F1 D275_01.jpg|280px]]
|[[Image:W15 MLA2 MiR F2 D275_03.jpg|280px]]
|[[Image:W15 MLA2 MiR F3 D275_01.jpg|280px]]
|[[Image:W15 MLA2 MiR F5 D275_01.jpg|280px]]


[[Image:MiR_Profile vs defoc.jpg|left|500px|thumb|Linewidth and sidewall angle vs. defocus value  for 1.5µm AZ MiR 701 exposed in Aligner: Maskless 02 (MLA2) using dose 275mJ/cm<sup>2</sup>. <br>Blue circles: Width of 2µm line. Orange Squares: Sidewall angle.]]
|-
|-style="background:WhiteSmoke; color:black"
|Lines
|[[Image:W15 MLA2 MiR F-1 D275_02.jpg|280px]]
|
|[[Image:W15 MLA2 MiR F2 D275_02.jpg|280px]]
|
|[[Image:W15 MLA2 MiR F5 D275_02.jpg|280px]]


|}
<br clear="all" />
<br clear="all" />


==AZ nLOF 2020==
==AZ nLOF 2020==
===Resolution===
<br clear="all" />
* Table with optimal parameters and resolution for different aligners
===Resolution (AZ nLOF 2020)===
* SEM pictures
<br clear="all" />
'''Resolution at optimal processing conditions for 2µm AZ nLOF 2020 using different exposure equipment:'''
{| class="wikitable"
|+
!Exposure equipment
!Dose [mJ/cm<sup>2</sup>]
!Contact/Defoc
!Resolution [µm]
!Comment
|-
|Aligner: MA6-2
|154
|Vacuum
|1
|
|-
|Aligner: Maskless 01 (MLA1)
|220
| -4
|2
|
|-
|Aligner: Maskless 02 (MLA2)
|450
|0
|1.25
|
|}
<br clear="all" />
 
'''SEM images of 2µm AZ nLOF 2020 from different exposure equipment at optimal processing conditions:'''


===Resist profile (sidewall angle and linewidth)===
{|border="1" cellspacing="0" cellpadding="3" style="text-align:left;"
*SEM pictures to support graphs?
|-


[[Image:nLOF_Linewidth vs dose.jpg|left|500px|thumb|Width of 2µm line vs. exposure dose for 2µm AZ nLOF 2020. <br>Blue circles: Exposed on Aligner: MA6-2 in vacuum contact. <br>Orange Squares: Exposed on Aligner: Maskless 01 (MLA1) using defoc -4 (QC defoc=-2). <br>Grey triangles: Exposed on Aligner: Maskless 02 (MLA2) using defoc 0 (QC defoc=2).]]
|-
|-style="background:silver; color:black"
!
!2µm triplets
!Lines
!Trenches
|-


[[Image:nLOF_Sidewall vs dose.jpg|left|500px|thumb|Sidewall angle vs. exposure dose for 2µm AZ nLOF 2020. <br>Blue circles: Exposed on Aligner: MA6-2 in vacuum contact. <br>Orange Squares: Exposed on Aligner: Maskless 01 (MLA1) using defoc -4 (QC defoc=-2). <br>Grey triangles: Exposed on Aligner: Maskless 02 (MLA2) using defoc 0 (QC defoc=2).]]
|-
|-style="background:WhiteSmoke; color:black"
|Aligner: MA6-2
154mJ/cm<sup>2</sup>, vacuum contact
|[[Image:W07 MA6 nLOF D154 vac C8T_01.jpg|400px]]
|[[Image:W07 MA6 nLOF D154 vac C8T_03.jpg|400px]]
|[[Image:W07 MA6 nLOF D154 vac C8T_04.jpg|400px]]


[[Image:nLOF_MLA1_Profile vs defoc.jpg|left|500px|thumb|Linewidth and sidewall angle vs. defocus value  for 2µm AZ nLOF exposed in Aligner: Maskless 01 (MLA1) using dose 220mJ/cm<sup>2</sup>. <br>Blue circles: Width of 2µm line. Orange Squares: Sidewall angle.]]  
|-
|-style="background:WhiteSmoke; color:black"
|Aligner: Maskless 01 (MLA1)
220mJ/cm<sup>2</sup>, Defoc -4
|[[Image:W06 MLA1 nLOF D220 F-4_2_01.jpg|400px]]
|[[Image:W06 MLA1 nLOF D220 F-4_2_03.jpg|400px]]
|[[Image:W06 MLA1 nLOF D220 F-4_2_04.jpg|400px]]


[[Image:nLOF_MLA2_Profile vs defoc.jpg|left|500px|thumb|Linewidth and sidewall angle vs. defocus value  for 2µm AZ nLOF exposed in Aligner: Maskless 02 (MLA2) using dose 450mJ/cm<sup>2</sup>. <br>Blue circles: Width of 2µm line. Orange Squares: Sidewall angle.]]
|-
|-style="background:WhiteSmoke; color:black"
|Aligner: Maskless 02 (MLA2)
450mJ/cm<sup>2</sup>, defoc 0
|[[Image:W17 mla2 nLOF D450 F0_04.jpg|400px]]
|[[Image:W17 mla2 nLOF D450 F0_03.jpg|400px]]
|[[Image:W17 mla2 nLOF D450 F0_02.jpg|400px]]


|}
<br clear="all" />
'''SEM images of different size structures for 2µm AZ nLOF 2020:'''
{|border="1" cellspacing="0" cellpadding="3" style="text-align:left;"
|-
|-
|-style="background:silver; color:black"
!
!1µm triplets
!2µm triplets
!4µm triplets
|-
|-
|-style="background:WhiteSmoke; color:black"
|Aligner: MA6-2
154mJ/cm<sup>2</sup>, vacuum contact
|[[Image:W07 MA6 nLOF D154 vac C8T_05.jpg|400px]]
|[[Image:W07 MA6 nLOF D154 vac C8T_01.jpg|400px]]
|[[Image:W07 MA6 nLOF D154 vac C8T_02.jpg|400px]]
|-
|-style="background:WhiteSmoke; color:black"
|Aligner: Maskless 01 (MLA1)
220mJ/cm<sup>2</sup>, Defoc -4
|[[Image:W06 MLA1 nLOF D220 F-4_02.jpg|400px]]
|[[Image:W06 MLA1 nLOF D220 F-4_2_01.jpg|400px]]
|[[Image:W06 MLA1 nLOF D220 F-4_03.jpg|400px]]
|}
<br clear="all" />
'''Cross-sectional SEM images of 2µm AZ nLOF 2020 at optimal processing conditions:'''
{|border="1" cellspacing="0" cellpadding="3" style="text-align:left;"
|-
|-
|-style="background:silver; color:black"
!
!2µm lines
!2µm trenches
!Lines
!Trenches
|-
|-
|-style="background:WhiteSmoke; color:black"
|Aligner: Maskless 01 (MLA1)
220mJ/cm<sup>2</sup>, Defoc -4
|[[Image:w04_mla1_nLOF_D220_F-4_X_l_2um.jpg|340px]]
|[[Image:w04_mla1_nLOF_D220_F-4_X_t_2um.jpg|340px]]
|[[Image:w04_mla1_nLOF_D220_F-4_Xlines.jpg|340px]]
|[[Image:w04_mla1_nLOF_D220_F-4_Xtrench.jpg|340px]]
|}
<br clear="all" />
===Resist profile (AZ nLOF 2020)===
<br clear="all" />
====Linewidth and sidewall angle vs exposure dose (AZ nLOF 2020)====
<br clear="all" />
'''Result of image analysis of SEM images of 2µm triplets:'''
{| cellpadding="2" style="border: 2px solid darkgray;" align="left"
! width="510" | 
|+
|- border="0" align="center"
|[[Image:nLOF_Linewidth vs dose.jpg|500px]]
|[[Image:nLOF_Sidewall vs dose.jpg|500px]]
|- align="center"
| colspan="2" | Sidewall angle vs. exposure dose for 2µm AZ nLOF 2020. <br>Blue circles: Exposed on Aligner: MA6-2 in vacuum contact. <br>Orange Squares: Exposed on Aligner: Maskless 01 (MLA1) using defoc -4 (QC defoc=-2). <br>Grey triangles: Exposed on Aligner: Maskless 02 (MLA2) using defoc 0 (QC defoc=2). 
|}
<br clear="all" />
'''SEM images of 2µm AZ nLOF 2020 as a function of exposure dose for Aligner: MA6-2 using vacuum contact:'''
{|border="1" cellspacing="0" cellpadding="3" style="text-align:left;"
|-
|-
|-style="background:silver; color:black"
!
!100mJ/cm<sup>2</sup>
!120mJ/cm<sup>2</sup>
!140mJ/cm<sup>2</sup>
!160mJ/cm<sup>2</sup>
|-
|-
|-style="background:WhiteSmoke; color:black"
|2µm triplets
|[[Image:w05_ma6_nLOF_D100_vac_2um.jpg|340px]]
|[[Image:w05_ma6_nLOF_D120_vac_2um.jpg|340px]]
|[[Image:w05_ma6_nLOF_D140_vac_2um.jpg|340px]]
|[[Image:w05_ma6_nLOF_D160_vac_2um.jpg|340px]]
|}
<br clear="all" />
'''SEM images of 2µm AZ nLOF 2020 as a function of exposure dose for Aligner: Maskless 01 (MLA1) using defoc -4:'''
{|border="1" cellspacing="0" cellpadding="3" style="text-align:left;"
|-
|-
|-style="background:silver; color:black"
!
!200mJ/cm<sup>2</sup>
!220mJ/cm<sup>2</sup>
!240mJ/cm<sup>2</sup>
|-
|-
|-style="background:WhiteSmoke; color:black"
|2µm triplets
|[[Image:w04_mla1_nLOF_D200_F-4_2um.jpg|340px]]
|[[Image:w04_mla1_nLOF_D220_F-4_2um.jpg|340px]]
|[[Image:w04_mla1_nLOF_D240_F-4_2um.jpg|340px]]
|}
<br clear="all" />
'''SEM images of 2µm AZ nLOF 2020 as a function of exposure dose for Aligner: Maskless 02 (MLA2) using defoc 0:'''
{|border="1" cellspacing="0" cellpadding="3" style="text-align:left;"
|-
|-
|-style="background:silver; color:black"
!
!400mJ/cm<sup>2</sup>
!450mJ/cm<sup>2</sup>
!500mJ/cm<sup>2</sup>
|-
|-
|-style="background:WhiteSmoke; color:black"
|2µm triplets
|[[Image:W17 mla2 nLOF D400 F0_01.jpg|340px]]
|[[Image:W17 mla2 nLOF D450 F0_04.jpg|340px]]
|[[Image:W17 mla2 nLOF D500 F0_01.jpg|340px]]
|}
<br clear="all" />
====Linewidth and sidewall angle vs defocus parameter (AZ nLOF 2020)====
<br clear="all" />
'''Result of image analysis of SEM images of 2µm triplets:'''
{| cellpadding="2" style="border: 2px solid darkgray;" align="left"
! width="510" | 
|+
|- border="0" align="center"
|[[Image:nLOF_MLA1_Profile vs defoc.jpg|500px]]
|[[Image:nLOF_MLA2_Profile vs defoc.jpg|500px]]
|- align="center"
| colspan="2" | Linewidth and sidewall angle vs. defocus value  for 2µm AZ nLOF <br>exposed in Aligner: Maskless 01 (MLA1) using dose 220mJ/cm<sup>2</sup> and Aligner: Maskless 02 (MLA2) using dose 450mJ/cm<sup>2</sup>, respectively. <br>Blue circles: Width of 2µm line. Orange Squares: Sidewall angle.
|}
<br clear="all" />
'''SEM images of 2µm AZ nLOF 2020 as a function of defocus parameter for Aligner: Maskless 01 (MLA1) using dose 220mJ/cm<sup>2</sup>:'''
{|border="1" cellspacing="0" cellpadding="3" style="text-align:left;"
|-
|-
|-style="background:silver; color:black"
!
!Defoc -14
!Defoc -7
!Defoc -4
!Defoc -1
!Defoc -6
|-
|-
|-style="background:WhiteSmoke; color:black"
|2µm triplets
|[[Image:W06 MLA1 nLOF D220 F-14_02.jpg|280px]]
|[[Image:W06 MLA1 nLOF D220 F-7_01.jpg|280px]]
|[[Image:W06 MLA1 nLOF D220 F-4_2_01.jpg|280px]]
|[[Image:W06 MLA1 nLOF D220 F-1_01.jpg|280px]]
|[[Image:W06 MLA1 nLOF D220 F6_02.jpg|280px]]
|-
|-style="background:WhiteSmoke; color:black"
|Lines
|[[Image:W06 MLA1 nLOF D220 F-14_03.jpg|280px]]
|[[Image:W06 MLA1 nLOF D220 F-7_03.jpg|280px]]
|[[Image:W06 MLA1 nLOF D220 F-4_2_03.jpg|280px]]
|[[Image:W06 MLA1 nLOF D220 F-1_03.jpg|280px]]
|[[Image:W06 MLA1 nLOF D220 F6_03.jpg|280px]]
|}
<br clear="all" />
'''SEM images of 2µm AZ nLOF 2020 as a function of defocus parameter for Aligner: Maskless 02 (MLA2) using dose 450mJ/cm<sup>2</sup>:'''
{|border="1" cellspacing="0" cellpadding="3" style="text-align:left;"
|-
|-
|-style="background:silver; color:black"
!
!Defoc 0
!Defoc 2
!Defoc 4
|-
|-
|-style="background:WhiteSmoke; color:black"
|2µm triplets
|[[Image:W17 mla2 nLOF D450 F0_04.jpg|340px]]
|[[Image:W17 mla2 nLOF D450 F2_01.jpg|340px]]
|[[Image:W17 mla2 nLOF D450 F4_02.jpg|340px]]
|-
|-style="background:WhiteSmoke; color:black"
|Lines
|[[Image:W17 mla2 nLOF D450 F0_03.jpg|340px]]
|[[Image:W17 mla2 nLOF D450 F2_02.jpg|340px]]
|[[Image:W17 mla2 nLOF D450 F4_03.jpg|340px]]
|}
<br clear="all" />
<br clear="all" />

Latest revision as of 14:55, 10 September 2026

The content on this page, including all images and pictures, was created by DTU Nanolab staff, unless otherwise stated.

Feedback to this page: click here

Mask Aligner vs Maskless Aligner

In the first half of 2026, a rather thorough investigation of the differences between exposure using mask aligner and maskless aligner was conducted. The result was presented as an advanced lithography tutorial at the 2026 Nordic Nanolab User Meeting in Uppsala, Sweden.

Slides presented at NNUM in Uppsala: MA6 vs MLA 2026_v09

Mask design used in the investigation: LithoTestAlign_2025_v10.gds

Tools used in the investigation


Data from the investigation


AZ 5214E


Resolution (AZ 5214E)


Resolution at optimal processing conditions for 1.5µm AZ 5214E using different exposure equipment:

Exposure equipment Dose [mJ/cm2] Contact/Defoc Resolution [µm] Comment
Aligner: MA6-2 100 Vacuum 1
Aligner: MA6-1 100 Vacuum 1.25 Probably over-exposed
Aligner: Maskless 02 (MLA2) 90 2 1.25


SEM images from different exposure equipment for 1.5µm AZ 5214E at optimal processing conditions:

2µm triplets Lines Trenches
Aligner: MA6-2

100mJ/cm2, vacuum contact

Aligner: MA6-1

100mJ/cm2, vacuum contact
(probably over-exposed)

Aligner: Maskless 02 (MLA2)

90mJ/cm2, defoc 2


SEM images of different size structures for 1.5µm AZ 5214E:

1µm triplets 2µm triplets 4µm triplets
Aligner: MA6-1

100mJ/cm2, vacuum contact
(probably over-exposed)


Yield (AZ 5214E)

The yield is measured by inspecting all 116 lithographic resolution test structures in an optical microscope and recording the smallest resolved dots and lines.

Wafer maps for 1.5µm AZ 5214E at optimal processing conditions for different aligners
Aligner: Maskless 02 (MLA2) (Dose 90mJ/cm2; defoc 2).
Resolution: 1.22µm average; 0.1µm standard deviation.
Yield at 1.25µm: 99%
Aligner: MA6-2 (Dose 100mJ/cm2; vacuum contact).
Resolution: 1.02µm average; 0.1µm standard deviation.
Yield at 1.25µm: 100%
Aligner: MA6-1 (Dose 100mJ/cm2; vacuum contact). Probably over-exposed.
Resolution: 1.30µm average; 0.2µm standard deviation.
Yield at 1.25µm: 59%


Effect of exposure mode for mask aligner

Wafer maps for 1.5µm AZ 5214E at different exposure modes for Aligner: MA6-2 (Dose 100mJ/cm2)
Hard contact.
Resolution: 1.17µm average; 0.2µm standard deviation.
Yield at 1.25µm: 89%
Soft contact.
Resolution: 3.77µm average; 0.7µm standard deviation.
Yield at 2.5µm: 4%
10µm proximity.
Resolution: 4.19µm average; 0.7µm standard deviation.
Yield at 2.5µm: 3%


Wafer maps for 1.5µm AZ 5214E at different exposure modes for Aligner: MA6-1 (Dose 100mJ/cm2, probably over-exposed)
Hard contact.
Resolution: 1.58µm average; 0.5µm standard deviation.
Yield at 1.25µm: 48%
Soft contact.
Resolution: 2.36µm average; 0.4µm standard deviation.
Yield at 2.5µm: 80%
At dose 92mJ/cm2, the average resolution decreases to 1.91µm and the yield at 2.5µm increases to 100%
10µm proximity.
Resolution: 2.73µm average; 0.6µm standard deviation.
Yield at 2.5µm: 53%


Effect of WEC pressure for mask aligner (after WEC head service)

Wafer maps for 1.5µm AZ 5214E at different WEC pressure for Aligner: MA6-2 (Dose 100mJ/cm2)
Soft contact, 0.15bar WEC pressure.
Resolution: 3.92µm average; 0.9µm standard deviation.
Yield at 2.5µm: 8%
Soft contact, 0.40bar WEC pressure.
Resolution: 2.19µm average; 0.5µm standard deviation.
Yield at 2.5µm: 86%
10µm proximity, 0.15bar WEC pressure.
Resolution: 3.22µm average; 0.8µm standard deviation.
Yield at 2.5µm: 34%
10µm proximity, 0.40bar WEC pressure.
Resolution: 2.83µm average; 0.6µm standard deviation.
Yield at 2.5µm: 66%


Resist profile (AZ 5214E)


Linewidth and sidewall angle vs exposure dose (AZ 5214E)


Result of image analysis of SEM images of 2µm triplets:

Width of 2µm line and sidewall angle vs. exposure dose for 1.5µm AZ 5214E.
Blue circles: Exposed on Aligner: MA6-2 in vacuum contact.
Orange Squares: Exposed on Aligner: Maskless 02 (MLA2) using defoc 2 (QC defoc=2).



SEM images of 1.5µm AZ 5214E as a function of exposure dose for Aligner: MA6-2 using vacuum contact:

85mJ/cm2 90mJ/cm2 95mJ/cm2 100mJ/cm2 105mJ/cm2
2µm triplets
Lines


SEM images of 1.5µm AZ 5214E as a function of exposure dose for Aligner: Maskless 02 (MLA2) using defoc 2:

80mJ/cm2 90mJ/cm2 100mJ/cm2 110mJ/cm2
2µm triplets
Trenches
and Lines


Linewidth and sidewall angle vs defocus parameter (AZ 5214E)


Result of image analysis of SEM images of 2µm triplets:

Linewidth and sidewall angle vs. defocus value for 1.5µm AZ 5214E exposed in Aligner: Maskless 02 (MLA2) using dose 95mJ/cm2.
Blue circles: Width of 2µm line.
Orange Squares: Sidewall angle.



SEM images of 1.5µm AZ 5214E as a function of defocus parameter for Aligner: Maskless 02 (MLA2) using dose 95mJ/cm2:

Defoc -8 Defoc -1 Defoc 2 Defoc 5 Defoc 12
2µm triplets
Lines


AZ MiR 701


Resolution (AZ MiR 701)


Resolution at optimal processing conditions for 1.5µm AZ MiR 701 using different exposure equipment:

Exposure equipment Dose [mJ/cm2] Contact/Defoc Resolution [µm] Comment
Aligner: MA6-2 220 Vacuum 1
Aligner: Maskless 02 (MLA2) 275 2 1


SEM images of 1.5µm AZ MiR 701 from different exposure equipment at optimal processing conditions:

2µm triplets Lines Trenches
Aligner: MA6-2

220mJ/cm2, vacuum contact

Aligner: Maskless 02 (MLA2)

275mJ/cm2, defoc 2


Resist profile (AZ MiR 701)


Linewidth and sidewall angle vs exposure dose (AZ MiR 701)


Result of image analysis of SEM images of 2µm triplets:

Width of 2µm line and sidewall angle vs. exposure dose for 1.5µm AZ MiR 701.
Blue circles: Exposed on Aligner: MA6-2 in vacuum contact.
Orange Squares: Exposed on Aligner: Maskless 02 (MLA2) using defoc 2 (QC defoc=2).



SEM images of 1.5µm AZ MiR 701 as a function of exposure dose for Aligner: MA6-2 using vacuum contact:

160mJ/cm2 190mJ/cm2 220mJ/cm2 250mJ/cm2 280mJ/cm2
2µm triplets
Lines


SEM images of 1.5µm AZ MiR 701 as a function of exposure dose for Aligner: Maskless 02 (MLA2) using defoc 2:

225mJ/cm2 275mJ/cm2 325mJ/cm2 375mJ/cm2
2µm triplets
Lines


Linewidth and sidewall angle vs defocus parameter (AZ MiR 701)


Result of image analysis of SEM images of 2µm triplets:

Linewidth and sidewall angle vs. defocus value for 1.5µm AZ MiR 701 exposed in Aligner: Maskless 02 (MLA2) using dose 95mJ/cm2.
Blue circles: Width of 2µm line.
Orange Squares: Sidewall angle.



SEM images of 1.5µm AZ MiR 701 as a function of defocus parameter for Aligner: Maskless 02 (MLA2) using dose 275mJ/cm2:

Defoc -1 Defoc 1 Defoc 2 Defoc 3 Defoc 5
2µm triplets
Lines


AZ nLOF 2020


Resolution (AZ nLOF 2020)


Resolution at optimal processing conditions for 2µm AZ nLOF 2020 using different exposure equipment:

Exposure equipment Dose [mJ/cm2] Contact/Defoc Resolution [µm] Comment
Aligner: MA6-2 154 Vacuum 1
Aligner: Maskless 01 (MLA1) 220 -4 2
Aligner: Maskless 02 (MLA2) 450 0 1.25


SEM images of 2µm AZ nLOF 2020 from different exposure equipment at optimal processing conditions:

2µm triplets Lines Trenches
Aligner: MA6-2

154mJ/cm2, vacuum contact

Aligner: Maskless 01 (MLA1)

220mJ/cm2, Defoc -4

Aligner: Maskless 02 (MLA2)

450mJ/cm2, defoc 0


SEM images of different size structures for 2µm AZ nLOF 2020:

1µm triplets 2µm triplets 4µm triplets
Aligner: MA6-2

154mJ/cm2, vacuum contact

Aligner: Maskless 01 (MLA1)

220mJ/cm2, Defoc -4


Cross-sectional SEM images of 2µm AZ nLOF 2020 at optimal processing conditions:

2µm lines 2µm trenches Lines Trenches
Aligner: Maskless 01 (MLA1)

220mJ/cm2, Defoc -4


Resist profile (AZ nLOF 2020)


Linewidth and sidewall angle vs exposure dose (AZ nLOF 2020)


Result of image analysis of SEM images of 2µm triplets:

Sidewall angle vs. exposure dose for 2µm AZ nLOF 2020.
Blue circles: Exposed on Aligner: MA6-2 in vacuum contact.
Orange Squares: Exposed on Aligner: Maskless 01 (MLA1) using defoc -4 (QC defoc=-2).
Grey triangles: Exposed on Aligner: Maskless 02 (MLA2) using defoc 0 (QC defoc=2).



SEM images of 2µm AZ nLOF 2020 as a function of exposure dose for Aligner: MA6-2 using vacuum contact:

100mJ/cm2 120mJ/cm2 140mJ/cm2 160mJ/cm2
2µm triplets



SEM images of 2µm AZ nLOF 2020 as a function of exposure dose for Aligner: Maskless 01 (MLA1) using defoc -4:

200mJ/cm2 220mJ/cm2 240mJ/cm2
2µm triplets



SEM images of 2µm AZ nLOF 2020 as a function of exposure dose for Aligner: Maskless 02 (MLA2) using defoc 0:

400mJ/cm2 450mJ/cm2 500mJ/cm2
2µm triplets


Linewidth and sidewall angle vs defocus parameter (AZ nLOF 2020)


Result of image analysis of SEM images of 2µm triplets:

Linewidth and sidewall angle vs. defocus value for 2µm AZ nLOF
exposed in Aligner: Maskless 01 (MLA1) using dose 220mJ/cm2 and Aligner: Maskless 02 (MLA2) using dose 450mJ/cm2, respectively.
Blue circles: Width of 2µm line. Orange Squares: Sidewall angle.



SEM images of 2µm AZ nLOF 2020 as a function of defocus parameter for Aligner: Maskless 01 (MLA1) using dose 220mJ/cm2:

Defoc -14 Defoc -7 Defoc -4 Defoc -1 Defoc -6
2µm triplets
Lines



SEM images of 2µm AZ nLOF 2020 as a function of defocus parameter for Aligner: Maskless 02 (MLA2) using dose 450mJ/cm2:

Defoc 0 Defoc 2 Defoc 4
2µm triplets
Lines