Jump to content

Specific Process Knowledge/Lithography/Aligners/Aligner: Maskless 03 processing: Difference between revisions

From LabAdviser
Jehem (talk | contribs)
Taran (talk | contribs)
 
(71 intermediate revisions by 3 users not shown)
Line 1: Line 1:
'''Feedback to this page''': '''[mailto:labadviser@danchip.dtu.dk?Subject=Feed%20back%20from%20page%20http://labadviser.danchip.dtu.dk/index.php/Specific_Process_Knowledge/Lithography/Aligners/Aligner:_Maskless_03_processing click here]'''
{{cc-nanolab}}


'''Feedback to this page''': '''[mailto:labadviser@nanolab.dtu.dk?Subject=Feed%20back%20from%20page%20http://labadviser.nanolab.dtu.dk/index.php?title=Specific_Process_Knowledge/Lithography/Aligners/Aligner:_Maskless_03_processing click here]'''
[[Category: Equipment|Lithography]]
[[Category: Lithography]]
__TOC__


=Exposure technology=
=Exposure technology=


Aligner: Maskless 03 is not a direct writer. In the maskless aligner, the exposure light is passed through a spatial light modulator, much like in a video projector, and projected onto the substrate, thus exposing an area of the design at a time. The substrate is exposed by scanning the exposure field across the substrate in a succession of stripes.
Aligner: Maskless 03 is ''not'' a direct laser writer. In the maskless aligner, the exposure light is passed through a spatial light modulator, much like in a video projector, and projected onto the substrate, exposing a small area of the design at a time. The substrate is fully exposed by scanning the exposure field across the substrate in a succession of exposure stripes.


The light source is a laser diode (array) with a wavelength of 405nm (8W). The spacial light modulator is a digital micro-mirror device. The individual mirrors of the DMD are switched in order to represent the design, and the laser is flashed in order to yield the desired exposure dose. This image is projected onto the substrate through a lens(system). The projected image yields a pixel size of 500nm X 500nm at wafer scale. The image is scanned across the substrate, in order to expose the entire design, each stripe overlapping (2 or 5 times depending on [[Specific_Process_Knowledge/Lithography/Aligners/Aligner:_Maskless_03_processing#Exposure_mode|exposure mode]]) in order to minimize uniformity effects and stitching errors. The address grid size is 250nm or 100nm for Fast or Quality exposure mode, respectively.
The light source is a laser diode (array) with a wavelength of 405 nm (8 W). The spatial light modulator is a digital micro-mirror device. The individual mirrors of the DMD are switched on and off in order to represent the design, and the laser is flashed on and off, in order to give the desired exposure dose. The exposure image is projected onto the substrate through a lens-system. The projected image has a pixel size of 500x500 nm on the substrate surface. The image is scanned across the substrate in stripes in order to expose the entire design. Each stripe is overlapping 2 or 5 times, depending on the chosen [[Specific_Process_Knowledge/Lithography/Aligners/Aligner:_Maskless_03_processing#Exposure_mode|exposure mode]]), in order to reduce light-source non-uniformity effects and stitching errors. The address grid size is 250 nm or 100 nm for Fast and High Quality exposure mode, respectively.
 
The writing head of the Aligner: Maskless 03 moves only in the z-direction. Using a pneumatic focusing system, the maskless aligner is able to do real-time autofocus. The defocus process parameter is used to compensate offsets in the focusing mechanism, and to optimize printing quality in different resists and varying thicknesses.
The stage of the Aligner: Maskless 03 moves only in x and y. It has no theta-axis. All rotation during alignment is thus accomplished by transformation of the input design.


The writing head of the Aligner: Maskless 03 moves only in the z-direction. Using the optical or pneumatic focusing system, the maskless aligner is able to do real-time dynamic autofocus. The defocus process parameter is used to offset the focusing mechanism, to optimize printing quality in different resists and resist thicknesses, as well as reflective or absorbing surfaces, and transparent or non-transparent substrates.
The stage of the Aligner: Maskless 03 moves only in x and y. It has no theta-axis. All rotation during alignment is accomplished by digitally rotating the design to match the physical rotation of the substrate.


=Process Parameters=
=Process Parameters=
Line 16: Line 21:


The correct way to determine the best dose-defocus settings is to generate a so-called Bossung plot (known from projection lithography), which plots the printed linewidth as a function of dose and defocus. From this, the most stable region of parameter space is chosen, i.e. the region where the linewidth changes the least when dose and defocus changes. Any deviation from the design linewidth may be corrected using the CD bias parameter. This typically involves SEM imaging of resist cross-sections, and quickly becomes time consuming. However, in most cases, inspection of a dose-defocus matrix (easily generated using the series exposure function) in an optical microscope will get you most of the way.  
The correct way to determine the best dose-defocus settings is to generate a so-called Bossung plot (known from projection lithography), which plots the printed linewidth as a function of dose and defocus. From this, the most stable region of parameter space is chosen, i.e. the region where the linewidth changes the least when dose and defocus changes. Any deviation from the design linewidth may be corrected using the CD bias parameter. This typically involves SEM imaging of resist cross-sections, and quickly becomes time consuming. However, in most cases, inspection of a dose-defocus matrix (easily generated using the series exposure function) in an optical microscope will get you most of the way.  
<br clear="all" />


'''Data represent dose-defocus tests on Si using optical autofocus unless otherwise stated'''
==Exposure dose and defocus==
 
[[Specific_Process_Knowledge/Lithography/Resist/UVresist/exposureDoseMasklessAligners#Aligner:_Maskless_03|Information on UV exposure dose]]
{|border="1" cellspacing="1" cellpadding="7" style="text-align:left;"
|-
 
|-
|-style="background:silver; color:black"
|
!Thickness
!Exposure mode
!Dose
!Defoc
!Resolution
!Comments
|-
 
|-
|-style="background:WhiteSmoke; color:black"
!rowspan="2"| AZ 5214E
|rowspan="2"| 1.5 µm
| Fast
| 69-72 mJ/cm<sup>2</sup>  (Taran Mar 2020)
| 0 (Jehem Feb 2020)
| 2 µm (due to stitching)
| Dev: SP60s
|-style="background:WhiteSmoke; color:black"
| Quality
| 69 mJ/cm<sup>2</sup> (Taran Mar 2020)
| 0 (Jehem Feb 2020)
| 1.25 µm
| Dev: SP60s
|-
 
|-
|-style="background:WhiteSmoke; color:black"
!rowspan="2"| AZ MiR 701
|rowspan="2"| 1.5 µm
| Fast
| 300 mJ/cm<sup>2</sup>  (Jehem Feb 2020)
| 0 (Jehem Feb 2020)
| 2 µm (due to stitching)
| PEB: 60s@110°C, Dev: SP60s
|-style="background:WhiteSmoke; color:black"
| Quality
| 180-200 mJ/cm<sup>2</sup> (Taran Mar 2020)
| 0-1 (Jehem Mar 2020)
| 1 µm
| PEB: 60s@110°C, Dev: SP60s
|-
 
|-
|-style="background:WhiteSmoke; color:black"
!rowspan="2"| AZ 5214E image reversal
|rowspan="2"| 2.2 µm
| Fast
| 43 mJ/cm<sup>2</sup> (Taran Mar 2020)
| 0 (Jehem Feb 2020)
| >2 µm (a lot of stitching)
| Reversal bake: 120s@110°C, Flood exposure: 200mJ/cm<sup>2</sup>, Dev: SP60s
|-style="background:WhiteSmoke; color:black"
| Quality
| 43 mJ/cm<sup>2</sup> (Taran Mar 2020)
| 0 (Jehem Feb 2020)
| 2 µm (due to stitching)
| Reversal bake: 120s@110°C, Flood exposure: 200mJ/cm<sup>2</sup>, Dev: SP60s
|-
 
|}
 
 
'''AZ nLOF 2020''' has also been tested. It seems to work even at 405nm, but the dose is so hign (>10000) that exposure would be slower than Aligner: Maskless 02.
 
<br clear="all" />


==Exposure mode==
==Exposure mode==
Line 95: Line 30:
Aligner: Maskless 03 offers two exposure modes. The exposure mode is selected during design conversion.
Aligner: Maskless 03 offers two exposure modes. The exposure mode is selected during design conversion.


'''Quality''' mode is used for optimal resolution, best overlay accuracy, and minimum stripe stitching effects.
'''Quality:'''


In the high quality mode, an area of the pattern is exposed by 5 stripes, each 500µm wide and exposing a fifth of the dose. At the same time, sub-pixel interpolation is applied, yielding an address grid size of 100nm.
Quality mode is used for optimal resolution, best overlay accuracy, and minimum stripe stitching effects.<br>
In the high quality mode, an area of the pattern is exposed by 5 stripes, each 500 µm wide and exposing a fifth of the dose. At the same time, sub-pixel interpolation is applied, yielding an address grid size of 100 nm.


'''Fast''' mode is used for maximum exposure speed.
'''Fast:'''


In the fast mode, each area of the pattern is exposed by 2 stripes only. This reduces the exposure time by 60%, but also increases the size of the address grid in the X-direction to 250nm. This means that alignment will be less accurate in fast mode. Due to less averaging of non-uniformities, stitching effects will be more prominent in this mode.
Fast mode is used for maximum exposure speed.<br>
In the fast mode, each area of the pattern is exposed by 2 stripes only. This reduces the exposure time by 60%, but also increases the size of the address grid in the x-direction to 250 nm. This means that alignment will be less accurate in fast mode. Due to less averaging of non-uniformities, stitching effects will be more prominent in this mode.


==Writing speed==
==Writing speed==
According to specs, the writing speed of Aligner: Maskless 03 is 1100mm<sup>2</sup>/min in fast mode. Using the high quality exposure mode cuts this speed in half, to approximately 550mm<sup>2</sup>/min. The writing speed for a 100x100mm<sup>2</sup> area measured during installation of the machine (acceptance test) was ~1200mm<sup>2</sup>/min.
According to specs, the writing speed of Aligner: Maskless 03 is 1100 mm<sup>2</sup>/min in fast mode. Using the high quality exposure mode reduces this speed to approximately 440 mm<sup>2</sup>/min. The writing speed for a 100 x 100 mm<sup>2</sup> area measured during installation of the machine (acceptance test) was ~1200 mm<sup>2</sup>/min.


[[Image:MLA3_speedVSarea.JPG|400x400px|thumb|The writing speed of Aligner: Maskless 03 as a function of the exposure area]]
[[Image:MLA3_speedVSarea.JPG|400x400px|thumb|The writing speed of Aligner: Maskless 03 as a function of the exposure area. Data and graph by Thomas Anhøj @ DTU Nanolab, 2020.]]




'''Speed vs. area:'''
'''Speed vs. area:'''


During exposure of a stripe the stage moves at a constant speed. Each stripe thus includes a certain movement overhead for acceleration and deceleration. As the stripes get shorter, this overhead becomes more significant, and the normal writing speed is no longer achieved. For samples slightly smaller than a 4" wafer, the writing speed of Aligner: Maskless 03 drops below the specified 1100mm<sup>2</sup>/min.
During exposure of a stripe the stage moves at a constant speed. Each stripe thus includes a certain movement overhead for acceleration and deceleration. As the stripes get shorter, this overhead becomes more significant, and the normal writing speed is no longer achieved. For samples slightly smaller than a 100 mm wafer, the writing speed of Aligner: Maskless 03 drops below the specified 1100 mm<sup>2</sup>/min.


When the exposure is started on the maskless aligner, the software starts converting the design to the data needed for the exposure. When sufficient data has been generated, the hardware starts exposing the sample while more data is being generated. This simultaneous data conversion and exposure is called Online conversion. Once a design has been converted (exposed) the data may be reused for repeated exposures (Offline conversion). However, the converted data can only be reused if no alignment is needed, including flat alignment ("Expose with substrate angle"). Due to the powerful, separate conversion PC on Aligner: Maskless 03, offline exposure is only very slightly faster than online.
When the exposure is started on the maskless aligner, the software starts converting the design to the data needed for the exposure. When sufficient data has been generated, the hardware starts exposing the sample while more data is being generated. This simultaneous data conversion and exposure is called Online conversion. Once a design has been converted (or exposed) the data may be reused for repeated exposures (Offline conversion). However, the converted data can only be reused if no alignment is needed, including flat alignment ("Expose with Global Angle"). Due to the powerful, separate conversion PC on Aligner: Maskless 03, offline exposure is only very slightly faster than online.


<br clear="all" />
<br clear="all" />


[[Image:MLA3_speedVSdose.JPG|400x400px|thumb|The writing speed of Aligner: Maskless 03 as a function of the exposure dose]]
[[Image:MLA3_speedVSdose.JPG|400x400px|thumb|The writing speed of Aligner: Maskless 03 as a function of the exposure dose. Data and graph by Thomas Anhøj @ DTU Nanolab, 2020.]]


'''Speed vs. dose:'''
'''Speed vs. dose:'''


The writing speed of Aligner: Maskless 03 remains constant up to a dose of 500mJ/cm<sup>2</sup>. After this point, the writing speed decreases with increasing dose. The writing speed is 50% at a dose around 2000mJ/cm<sup>2</sup>.
The writing speed of Aligner: Maskless 03 remains constant up to a dose of 500 mJ/cm<sup>2</sup>. After this point, the writing speed decreases with increasing dose. The writing speed is 50% at a dose around 2000 mJ/cm<sup>2</sup>.


<br clear="all" />
<br clear="all" />
Line 127: Line 64:
==Acceptance test==
==Acceptance test==


Acceptance criteria on a 100 X 100 mm<sup>2</sup> area: Width of smallest resolved line 1000±120 nm (quality), alignment error 500 nm (quality), writing speed 1100 mm<sup>2</sup>/min (fast).
Acceptance criteria on a 100 X 100 mm<sup>2</sup> area: Width of smallest resolved line 1000 ±120 nm (quality) in 0.5µm resist, alignment error 500 nm (quality), writing speed 1100 mm<sup>2</sup>/min (fast).


The acceptance test also included a verification of back side alignment (better than 1 µm), as well as a test of the conversion speed (less than 15 minutes for a dense design of circles).
The acceptance test also included a verification of back side alignment (better than 1 µm), as well as a test of the conversion speed (less than 15 minutes for a dense design of circles).


'''Exposed on mask blank, transferred via wet chrome etch, and measured at Heidelberg (FAT), or exposed and inspected at DTU (SAT)'''
'''Exposed on mask blank, transferred via wet chrome etch, and measured at Heidelberg (FAT), or exposed and inspected at DTU (SAT) (both 0.5µm resist)'''


{|border="1" cellspacing="0" cellpadding="3" style="text-align:center;"  
{|border="1" cellspacing="0" cellpadding="3" style="text-align:center;"  
Line 175: Line 112:
At the end of substrate detection, the sample is scanned twice along the bottom edge (flat), in order to determine the substrate rotation. This angle will be presented in the exposure panel along with the option to expose the design rotated in order to compensate for this angle, i.e. aligned to the flat/edge of the substrate.
At the end of substrate detection, the sample is scanned twice along the bottom edge (flat), in order to determine the substrate rotation. This angle will be presented in the exposure panel along with the option to expose the design rotated in order to compensate for this angle, i.e. aligned to the flat/edge of the substrate.


'''Result of using "Expose with substrate angle":'''  
'''Result of using "Expose with Global Angle":'''  
*Rotation: 0.05±0.2°
*Rotation: 0.05 ±0.2°
*Centering:
*Centering:
** '''X''' -125±25µm
** '''X''' -125 ±25 µm
** '''Y''' 104±36µm
** '''Y''' 104 ±36 µm
Jehem Feb 2020, average of 3 4" wafers.
Jehem Feb 2020, average of 3 100 mm wafers.




Line 197: Line 134:
|-style="background:WhiteSmoke; color:black"
|-style="background:WhiteSmoke; color:black"
|Jehem Feb 2020
|Jehem Feb 2020
| 3.6 mRad
| 3.6 mrad
| ±1.4 mRad
| ±1.4 mrad
±0.08°
±0.08°


Line 204: Line 141:




As expected from Aligner Maskless 01 and 02, the accuracy of flat alignment is ±0.1°, and the substrate centering is within a couple of hundred µm.
As expected from MLA1 and MLA2, the accuracy of flat alignment on MLA3 is ±0.1°, and the substrate centering is within a couple of hundred µm.
 
==Labeling==
 
[[Image:MLA150_label.JPG|400x400px|thumb|An example of wafer ID produced by the labeling function. Photograph by Thomas Anhøj @ DTU Nanolab, 2019.]]
 
The conversion manager software allows for inclusion of labels during the design conversion process. The labels are configured in a .lbl tab-delimited ASCII file with a special header in the first row, which must be located in the '...\Designs\Labels' folder. When used, the labels defined in the label file will be merged with the pattern in the source file, and the result can be inspected in the viewer. The X and Y positions of the labels should be given in design coordinates, and will be subject to any offsets/shifts applied to the design. Note, that if the label file is changed, the job file will not update automatically.
 
'''Example of a label file:'''
 
X | Y | UNIT | HEIGHT | UNIT | TITLE
 
-16000 | -46000 | um | 2000 | um | TARAN DTU Nanolab 20190320
 
This produces a 2 mm high, approximately 32 mm long wafer ID at the flat of a 100 mm wafer. Some special characters are not allowed (eg. ';').
 
<br clear="all" />


==Large defocus range==
==Large defocus range==


The standard range for the defocus parameter is -10 to 10, but a special feature allows to extend this range to -25 to 25, which may be useful when exposing thick resist. The large defocus range feature is activated in the resist template, and can only be accessed by asking staff to set up a custom resist template.
The standard range for the defocus parameter is -10 to 10, but a special feature allows to extend this range to -25 to 25, which may be useful when exposing thick resist. The large defocus range feature is set in the resist template, and can only be accessed by choosing the 'Special - Large defoc range' resist template during the job setup. The dose must be set manually, as this is an otherwise empty resist template.
 
<br clear="all" />
 
==CD Bias==
[[Image:MLA3_5214E_3umLS_bias.JPG|400x400px|thumb|The effect of applying CD Bias during conversion on Aligner: Maskless 03. Data and graph by Thomas Anhøj @ DTU Nanolab, 2023.]]
 
The size after development of the structures printed on Aligner: Maskless 03 is not necessarily 1:1 with the design. Tests have shown that 3µm lines of resist printed in positive resist using quality mode on Aligner: Maskless 03 resist are 0.4 - 0.8 µm too narrow, i.e. the exposed and subsequently developed area is wider than in the design. The bias is a function of the dose, and gets bigger with higher dose. It is also different for different resists. At the dose that appears to give the best resolution for AZ 5214E, the bias is 0.7 µm, while it is approximately 0.45 µm for AZ MiR 701.
 
The conversion manager software allows for correction of CD bias during the design conversion process. This correction is separate for the X- and Y-direction, but only in 200 nm steps, and only negative values, i.e. decreasing the exposed area. In the X-direction, the step size changes with the exposure mode, so CD bias correction probably only makes sense for quality mode exposures. From tests, see also figure to the right, it seems that applying a -200 nm CD bias makes a printed resist line 0.2 µm wider, so the CD bias correction apparently works by decreasing all structures by one sub-pixel (which for MLA3 in quality mode corresponds to 100 nm, as it prints 5-over using 500 nm pixels).  
 
<br clear="all" />


=Alignment=
=Alignment=


'''This section is under construction [[Image:section under construction.jpg|70px]]'''
In order to get good alignment, it is advised to use four alignment marks for alignment, and to activate scaling (possibly also shearing) before starting the exposure. It is recommended to use the "High Res" camera for the final alignment of each mark in order to achieve the best overlay accuracy. Exposure using the fast mode decreases the overlay accuracy, since the address grid size is increased to 250 nm.


==Top Side Alignment==
==Top Side Alignment==


'''Overlay accuracy (spec):''' 0.5µm
'''Overlay accuracy (spec):''' 0.5 µm


'''Camera field of view (W x H):''' <br>
'''Camera field of view (W x H):''' <br>
'''High Res''' ??µm x ??µm <br>
'''High Res''' 190 µm x 140 µm <br>
'''Low Res''' ??µm x ??µm <br>
'''Low Res''' 640 µm x 480 µm <br>
'''Overview''' 13mm x 10mm
'''Overview''' 12 mm x 9 mm


'''Accessible stage coordinates:''' <br>
'''Accessible stage coordinates:''' <br>
'''High/Low Res''' X = ±??mm; Y = ±??mm <br>
'''High/Low Res''' X = ±106 mm; Y = ±108 mm <br>
'''Overview''' X = ±??mm; Y = +10?mm to -??mm <br>
'''Overview''' X = ±104 mm; Y = +35 mm to -182 mm <br>
To be sure the Overview camera can be used to locate the first alignment mark, it is advised to use a mark in the bottom left portion (3<sup>rd</sup> quadrant) of the design as mark 1. <br>
To be sure the Overview camera can be used to locate the first alignment mark, it is advised to use a mark in the bottom left portion (3<sup>rd</sup> quadrant) of the design as mark 1. <br>
{| cellpadding="2" style="border: 2px solid darkgray;" align="center"
! width="320" |
! width="320" |
! width="320" |
|+'''Camera views during alignment on Aligner: Maskless 03. Screenshots by Thomas Anhøj @ DTU Nanolab, 2019.'''
|- border="0"; align="center"
|[[Image:MLA150 TSA Overview.JPG|300px]]
|[[Image:MLA150_BSA_Backside.JPG|300px]]
|[[Image:MLA150_TSA_Low_Res.JPG|300px]]
|- align="center"
| Overview camera image of a TSA alignment mark during alignment.<br/> The circle is 3 mm in diameter, the alignment mark is 300 µm. The blue cross-hair is ~400 µm. ||  Low Res camera image of a TSA alignment mark during alignment.<br/> The mark is 300 µm wide. The blue cross-hair is ~18 µm. || High Res camera image of a TSA alignment mark during alignment.<br/> The lines of the cross are 20 µm wide. The blue cross-hair is ~7 µm.
|}
<br clear="all" />


==Back Side Alignment==
==Back Side Alignment==


'''Overlay accuracy (spec):''' 1.0µm
'''Overlay accuracy (spec):''' 1.0 µm
 
'''BSA windows:''' along the X and Y axes, 10 mm x 46 mm, starting 14.5 mm from the center.
 
'''Camera field of view (W x H):''' 640 µm x 480 µm
 
[[Image:MLA150_BSA_Backside.JPG|center|300px|thumb|Image of a BSA alignment mark during alignment. The mark is 300 µm wide. The blue cross-hair is ~18 µm. Screenshot by Thomas Anhøj @ DTU Nanolab, 2019.]]
 
 
The alignment marks must be placed within the BSA windows. The Overview camera only shows the top side of the substrate, and cannot be used to locate the BSA marks.
 
{| cellpadding="2" style="border: 2px solid darkgray;" align="center"
! width="320" |
! width="320" |
! width="320" |
 
 
|+'''Substrate view during backside alignment. Screenshots by Thomas Anhøj @ DTU Nanolab, 2019.'''
|- border="0" align="center"
|[[Image:MLA150 BSA 2inch.JPG|300px]]
|[[Image:MLA150_BSA_4inch.JPG|300px]]
|[[Image:MLA150_BSA_6inch_mod.jpg|300px]]
 
|- align="center"
| BSA marks positioned at x = ±20 mm on a 2" wafer ||  BSA marks positioned at x = ±40 mm on a 100 mm wafer || BSA marks positioned at x = ±50 mm on a 150 mm wafer


'''BSA windows:''' along the X and Y axes, 10mm x 46mm, starting 14.5mm from the center.
|}


'''Camera field of view (W x H):''' 640µm x 480µm
<br clear="all" />
<br clear="all" />


==Advanced Field alignment (TSA)==
==Advanced Field alignment (TSA)==


'''Overlay accuracy (spec):''' 0.25µm (5x5mm<sup>2</sup> area)
'''Overlay accuracy (spec):''' 0.25 µm (5x5 mm<sup>2</sup> area)


Shift, rotation, scaling, and shearing is determined and set by global alignment marks. The shift is corrected by automatic alignment to one mark in each field (chip).
Shift, rotation, scaling, and shearing is determined and set by global alignment marks. The shift is corrected by automatic alignment to one mark in each field (chip).


'''Advanced field alignment test:'''
{|border="1" cellspacing="0" cellpadding="3" style="text-align:left;"  
{|border="1" cellspacing="0" cellpadding="3" style="text-align:left;"  
|-
|-
Line 249: Line 255:
|-style="background:silver; color:black"
|-style="background:silver; color:black"
!colspan="2" align="center"|
!colspan="2" align="center"|
!Shift (median) [nm]
!Median [nm]
!Error (average) [nm]
!Average [nm]
|-
|-


Line 260: Line 266:
(Jehem Feb 2020)
(Jehem Feb 2020)
|'''X'''
|'''X'''
|  
| 100 ±55
| 106±55
| 106 ±55


|-
|-
|-style="background:WhiteSmoke; color:black"
|-style="background:WhiteSmoke; color:black"
|'''Y'''
|'''Y'''
|  
| 100 ±56
| 104±56
| 104 ±56


|}
|}


<br clear="all" />
<br clear="all" />

Latest revision as of 10:10, 21 August 2026

The content on this page, including all images and pictures, was created by DTU Nanolab staff, unless otherwise stated.

Feedback to this page: click here

Exposure technology

Aligner: Maskless 03 is not a direct laser writer. In the maskless aligner, the exposure light is passed through a spatial light modulator, much like in a video projector, and projected onto the substrate, exposing a small area of the design at a time. The substrate is fully exposed by scanning the exposure field across the substrate in a succession of exposure stripes.

The light source is a laser diode (array) with a wavelength of 405 nm (8 W). The spatial light modulator is a digital micro-mirror device. The individual mirrors of the DMD are switched on and off in order to represent the design, and the laser is flashed on and off, in order to give the desired exposure dose. The exposure image is projected onto the substrate through a lens-system. The projected image has a pixel size of 500x500 nm on the substrate surface. The image is scanned across the substrate in stripes in order to expose the entire design. Each stripe is overlapping 2 or 5 times, depending on the chosen exposure mode), in order to reduce light-source non-uniformity effects and stitching errors. The address grid size is 250 nm or 100 nm for Fast and High Quality exposure mode, respectively.

The writing head of the Aligner: Maskless 03 moves only in the z-direction. Using the optical or pneumatic focusing system, the maskless aligner is able to do real-time dynamic autofocus. The defocus process parameter is used to offset the focusing mechanism, to optimize printing quality in different resists and resist thicknesses, as well as reflective or absorbing surfaces, and transparent or non-transparent substrates. The stage of the Aligner: Maskless 03 moves only in x and y. It has no theta-axis. All rotation during alignment is accomplished by digitally rotating the design to match the physical rotation of the substrate.

Process Parameters

The lithographic result of exposure on Aligner: Maskless 03 depends on a lot of factors, including the dose and defocus parameters, and the exposure mode used. The optimal dose and defocus depend on the type and thickness of the resist, and the optical properties of the substrate (e.g. reflective/absorbing/transparent). All of these factors influence the obtainable resolution, as well as the writing speed.

The correct way to determine the best dose-defocus settings is to generate a so-called Bossung plot (known from projection lithography), which plots the printed linewidth as a function of dose and defocus. From this, the most stable region of parameter space is chosen, i.e. the region where the linewidth changes the least when dose and defocus changes. Any deviation from the design linewidth may be corrected using the CD bias parameter. This typically involves SEM imaging of resist cross-sections, and quickly becomes time consuming. However, in most cases, inspection of a dose-defocus matrix (easily generated using the series exposure function) in an optical microscope will get you most of the way.

Exposure dose and defocus

Information on UV exposure dose

Exposure mode

Aligner: Maskless 03 offers two exposure modes. The exposure mode is selected during design conversion.

Quality:

Quality mode is used for optimal resolution, best overlay accuracy, and minimum stripe stitching effects.
In the high quality mode, an area of the pattern is exposed by 5 stripes, each 500 µm wide and exposing a fifth of the dose. At the same time, sub-pixel interpolation is applied, yielding an address grid size of 100 nm.

Fast:

Fast mode is used for maximum exposure speed.
In the fast mode, each area of the pattern is exposed by 2 stripes only. This reduces the exposure time by 60%, but also increases the size of the address grid in the x-direction to 250 nm. This means that alignment will be less accurate in fast mode. Due to less averaging of non-uniformities, stitching effects will be more prominent in this mode.

Writing speed

According to specs, the writing speed of Aligner: Maskless 03 is 1100 mm2/min in fast mode. Using the high quality exposure mode reduces this speed to approximately 440 mm2/min. The writing speed for a 100 x 100 mm2 area measured during installation of the machine (acceptance test) was ~1200 mm2/min.

The writing speed of Aligner: Maskless 03 as a function of the exposure area. Data and graph by Thomas Anhøj @ DTU Nanolab, 2020.


Speed vs. area:

During exposure of a stripe the stage moves at a constant speed. Each stripe thus includes a certain movement overhead for acceleration and deceleration. As the stripes get shorter, this overhead becomes more significant, and the normal writing speed is no longer achieved. For samples slightly smaller than a 100 mm wafer, the writing speed of Aligner: Maskless 03 drops below the specified 1100 mm2/min.

When the exposure is started on the maskless aligner, the software starts converting the design to the data needed for the exposure. When sufficient data has been generated, the hardware starts exposing the sample while more data is being generated. This simultaneous data conversion and exposure is called Online conversion. Once a design has been converted (or exposed) the data may be reused for repeated exposures (Offline conversion). However, the converted data can only be reused if no alignment is needed, including flat alignment ("Expose with Global Angle"). Due to the powerful, separate conversion PC on Aligner: Maskless 03, offline exposure is only very slightly faster than online.


The writing speed of Aligner: Maskless 03 as a function of the exposure dose. Data and graph by Thomas Anhøj @ DTU Nanolab, 2020.

Speed vs. dose:

The writing speed of Aligner: Maskless 03 remains constant up to a dose of 500 mJ/cm2. After this point, the writing speed decreases with increasing dose. The writing speed is 50% at a dose around 2000 mJ/cm2.


Acceptance test

Acceptance criteria on a 100 X 100 mm2 area: Width of smallest resolved line 1000 ±120 nm (quality) in 0.5µm resist, alignment error 500 nm (quality), writing speed 1100 mm2/min (fast).

The acceptance test also included a verification of back side alignment (better than 1 µm), as well as a test of the conversion speed (less than 15 minutes for a dense design of circles).

Exposed on mask blank, transferred via wet chrome etch, and measured at Heidelberg (FAT), or exposed and inspected at DTU (SAT) (both 0.5µm resist)

Width of smallest resolved line [nm] Alignment error (TSA) [nm] Exposure speed [mm2/min]
FAT December 2019 X 985±72 427 1269
Y 953±47 362
SAT February 2020 ≤1000 ≤500 1212

Features

Substrate centring and flat alignment

During substrate detection, the sample is scanned along the X- and Y-axes, as well as diagonally. From these measurements, the size (diameter) of the substrate is calculated, as well as the stage position matching the center of the substrate. This stage position will be the default origin for the subsequent exposure.

At the end of substrate detection, the sample is scanned twice along the bottom edge (flat), in order to determine the substrate rotation. This angle will be presented in the exposure panel along with the option to expose the design rotated in order to compensate for this angle, i.e. aligned to the flat/edge of the substrate.

Result of using "Expose with Global Angle":

  • Rotation: 0.05 ±0.2°
  • Centering:
    • X -125 ±25 µm
    • Y 104 ±36 µm

Jehem Feb 2020, average of 3 100 mm wafers.


Result of loading the same substrate 10 times without removing it from the stage:

Average Range
Jehem Feb 2020 3.6 mrad ±1.4 mrad

±0.08°


As expected from MLA1 and MLA2, the accuracy of flat alignment on MLA3 is ±0.1°, and the substrate centering is within a couple of hundred µm.

Labeling

An example of wafer ID produced by the labeling function. Photograph by Thomas Anhøj @ DTU Nanolab, 2019.

The conversion manager software allows for inclusion of labels during the design conversion process. The labels are configured in a .lbl tab-delimited ASCII file with a special header in the first row, which must be located in the '...\Designs\Labels' folder. When used, the labels defined in the label file will be merged with the pattern in the source file, and the result can be inspected in the viewer. The X and Y positions of the labels should be given in design coordinates, and will be subject to any offsets/shifts applied to the design. Note, that if the label file is changed, the job file will not update automatically.

Example of a label file:

X | Y | UNIT | HEIGHT | UNIT | TITLE

-16000 | -46000 | um | 2000 | um | TARAN DTU Nanolab 20190320

This produces a 2 mm high, approximately 32 mm long wafer ID at the flat of a 100 mm wafer. Some special characters are not allowed (eg. ';').


Large defocus range

The standard range for the defocus parameter is -10 to 10, but a special feature allows to extend this range to -25 to 25, which may be useful when exposing thick resist. The large defocus range feature is set in the resist template, and can only be accessed by choosing the 'Special - Large defoc range' resist template during the job setup. The dose must be set manually, as this is an otherwise empty resist template.


CD Bias

The effect of applying CD Bias during conversion on Aligner: Maskless 03. Data and graph by Thomas Anhøj @ DTU Nanolab, 2023.

The size after development of the structures printed on Aligner: Maskless 03 is not necessarily 1:1 with the design. Tests have shown that 3µm lines of resist printed in positive resist using quality mode on Aligner: Maskless 03 resist are 0.4 - 0.8 µm too narrow, i.e. the exposed and subsequently developed area is wider than in the design. The bias is a function of the dose, and gets bigger with higher dose. It is also different for different resists. At the dose that appears to give the best resolution for AZ 5214E, the bias is 0.7 µm, while it is approximately 0.45 µm for AZ MiR 701.

The conversion manager software allows for correction of CD bias during the design conversion process. This correction is separate for the X- and Y-direction, but only in 200 nm steps, and only negative values, i.e. decreasing the exposed area. In the X-direction, the step size changes with the exposure mode, so CD bias correction probably only makes sense for quality mode exposures. From tests, see also figure to the right, it seems that applying a -200 nm CD bias makes a printed resist line 0.2 µm wider, so the CD bias correction apparently works by decreasing all structures by one sub-pixel (which for MLA3 in quality mode corresponds to 100 nm, as it prints 5-over using 500 nm pixels).


Alignment

In order to get good alignment, it is advised to use four alignment marks for alignment, and to activate scaling (possibly also shearing) before starting the exposure. It is recommended to use the "High Res" camera for the final alignment of each mark in order to achieve the best overlay accuracy. Exposure using the fast mode decreases the overlay accuracy, since the address grid size is increased to 250 nm.

Top Side Alignment

Overlay accuracy (spec): 0.5 µm

Camera field of view (W x H):
High Res 190 µm x 140 µm
Low Res 640 µm x 480 µm
Overview 12 mm x 9 mm

Accessible stage coordinates:
High/Low Res X = ±106 mm; Y = ±108 mm
Overview X = ±104 mm; Y = +35 mm to -182 mm
To be sure the Overview camera can be used to locate the first alignment mark, it is advised to use a mark in the bottom left portion (3rd quadrant) of the design as mark 1.

Camera views during alignment on Aligner: Maskless 03. Screenshots by Thomas Anhøj @ DTU Nanolab, 2019.
Overview camera image of a TSA alignment mark during alignment.
The circle is 3 mm in diameter, the alignment mark is 300 µm. The blue cross-hair is ~400 µm.
Low Res camera image of a TSA alignment mark during alignment.
The mark is 300 µm wide. The blue cross-hair is ~18 µm.
High Res camera image of a TSA alignment mark during alignment.
The lines of the cross are 20 µm wide. The blue cross-hair is ~7 µm.


Back Side Alignment

Overlay accuracy (spec): 1.0 µm

BSA windows: along the X and Y axes, 10 mm x 46 mm, starting 14.5 mm from the center.

Camera field of view (W x H): 640 µm x 480 µm

Image of a BSA alignment mark during alignment. The mark is 300 µm wide. The blue cross-hair is ~18 µm. Screenshot by Thomas Anhøj @ DTU Nanolab, 2019.


The alignment marks must be placed within the BSA windows. The Overview camera only shows the top side of the substrate, and cannot be used to locate the BSA marks.


Substrate view during backside alignment. Screenshots by Thomas Anhøj @ DTU Nanolab, 2019.
BSA marks positioned at x = ±20 mm on a 2" wafer BSA marks positioned at x = ±40 mm on a 100 mm wafer BSA marks positioned at x = ±50 mm on a 150 mm wafer


Advanced Field alignment (TSA)

Overlay accuracy (spec): 0.25 µm (5x5 mm2 area)

Shift, rotation, scaling, and shearing is determined and set by global alignment marks. The shift is corrected by automatic alignment to one mark in each field (chip).

Advanced field alignment test:

Median [nm] Average [nm]
25 fields

High res camera

(Jehem Feb 2020)

X 100 ±55 106 ±55
Y 100 ±56 104 ±56