Jump to content

Specific Process Knowledge/Lithography/Baking: Difference between revisions

From LabAdviser
Jehem (talk | contribs)
Thes (talk | contribs)
No edit summary
 
(31 intermediate revisions by 3 users not shown)
Line 1: Line 1:
'''Feedback to this page''': '''[mailto:photolith@danchip.dtu.dk?Subject=Feed%20back%20from%20page%20http://labadviser.danchip.dtu.dk/index.php/Specific_Process_Knowledge/Lithography/Baking click here]'''
{{cc-nanolab}}


[[Category: Equipment |Lithography baking]]
'''Feedback to this page''': '''[mailto:labadviser@nanolab.dtu.dk?Subject=Feed%20back%20from%20page%20https://labadviser.nanolab.dtu.dk/index.php?title=Specific_Process_Knowledge/Lithography/Baking click here]'''
 
[[Category: Equipment|baking]]
[[Category: Lithography|Baking]]
[[Category: Lithography|Baking]]
__TOC__


=Comparing baking methods=
=Comparing baking methods=


{|border="1" cellspacing="1" cellpadding="3" style="text-align:left;"  
{|border="1" cellspacing="1" cellpadding="10" style="text-align:left;"  
|-
|-


Line 13: Line 17:
!
!
![[Specific_Process_Knowledge/Lithography/Baking#Small benchtop hotplates|Spray coater hotplate]]
![[Specific_Process_Knowledge/Lithography/Baking#Small benchtop hotplates|Spray coater hotplate]]
![[Specific_Process_Knowledge/Lithography/Baking#Hotplate_1_.28SU8.29.2C_Hotplate_2_.28SU8.29.2C_Hoplate_3.28SU8.29_and_Hotplate_4.28SU8.29|SU8 hotplates 1, 2 and 3]]
![[Specific_Process_Knowledge/Lithography/Baking#SU-8 hotplates| SU-8 hotplates<br>(1 & 2 + 3 & 4)]]
![[Specific Process Knowledge/Lithography/Baking#Small_benchtop_hotplates|Small benchtop hotplates]]
![[Specific Process Knowledge/Lithography/Baking#Small_benchtop_hotplates|Small benchtop hotplates]]
![[Specific Process Knowledge/Lithography/Baking#Gamma_hotplates|Gamma hotplates]]
![[Specific Process Knowledge/Lithography/Baking#Gamma_hotplates|Gamma hotplates]]
![[Specific_Process_Knowledge/Lithography/Baking#Oven 90C|Oven 90C]]
![[Specific_Process_Knowledge/Lithography/Baking#Oven: 110C - 250C|Oven: 110C - 250C]]
![[Specific_Process_Knowledge/Lithography/Baking#Oven: 110C - 250C|Oven: 110C - 250C]]
![[Specific Process Knowledge/Lithography/Pretreatment#Oven 250C|Oven 250C]]
![[Specific Process Knowledge/Lithography/Baking#Oven_250C|Oven 250C]]
|-
|-


Line 50: Line 53:
*PEB
*PEB
*Hard bake
*Hard bake
|
Manual convection bake
*Soft bake
|
|
Manual convection bake
Manual convection bake
Line 71: Line 71:
Temperature with top-plate: Actual surface temperature = 0.9 * display value
Temperature with top-plate: Actual surface temperature = 0.9 * display value
|
|
Maximum 110°C
Maximum 180°C
|
|
Hotplate: 90-110C:<br />
Hotplate: 90-110C:<br />
Line 83: Line 83:
|
|
Fixed at various recipe dependent temperatures
Fixed at various recipe dependent temperatures
|
Fixed at 90°C
|
|
110 - 250°C
110 - 250°C
Line 114: Line 112:
* 150 mm wafer
* 150 mm wafer
* 200 mm wafer
* 200 mm wafer
|
* 100 mm wafers
* 150 mm wafers
|
|
* 100 mm wafers
* 100 mm wafers
Line 143: Line 138:
(All substrates and film or pattern of all types, unless otherwise noted on the hotplate)
(All substrates and film or pattern of all types, unless otherwise noted on the hotplate)
|
|
Silicon and glass substrates
Tool dependent. Typically Silicon, III-V, and glass substrates.
|
Silicon, glass, and polymer substrates
 
Film or pattern of all types
|
|
Silicon, glass, and high Tg polymer substrates
Silicon, glass, and high Tg polymer substrates
Line 155: Line 146:
Silicon, glass, and high Tg polymer substrates
Silicon, glass, and high Tg polymer substrates


Film or pattern of all types except resist|
Film or pattern of all types except resist
|-
|-


Line 168: Line 159:
Hotplate dependent. Any restrictions will be noted on the hotplate.
Hotplate dependent. Any restrictions will be noted on the hotplate.
|
|
Low Tg polymer, copper, steel substrates.


|III-V, copper, steel substrates
Pb, Te films.
|III-V, low Tg polymer, copper, steel substrates
|III-V, low Tg polymer, copper, steel substrates
|III-V, low Tg polymer, copper, steel substrates
|III-V, low Tg polymer, copper, steel substrates
Line 179: Line 171:
|-style="background:WhiteSmoke; color:black"  
|-style="background:WhiteSmoke; color:black"  
|- valign="top"
|- valign="top"
!QC
!QC<br>'''- requires login'''
|
|
https://labmanager.dtu.dk/view_binary.php?type=data&mach=293
https://labmanager.dtu.dk/view_binary.php?type=data&mach=293
Line 187: Line 179:


Hotplate 2:<br /> https://labmanager.dtu.dk/view_binary.php?type=data&mach=124  
Hotplate 2:<br /> https://labmanager.dtu.dk/view_binary.php?type=data&mach=124  
 
Hotplate 3:<br /> https://labmanager.dtu.dk/view_binary.php?type=data&mach=453


|
|
Line 198: Line 189:


|
|
Spincoater: Gamma ebeam & UV:<br />  http://labmanager.dtu.dk/view_binary.php?fileId=4431
Spincoater: Gamma ebeam & UV:<br />  https://labmanager.dtu.dk/view_binary.php?type=data&mach=417


Spincoater: Gamma UV:<br />  http://labmanager.dtu.dk/view_binary.php?fileId=4432
Spincoater: Gamma UV:<br />  https://labmanager.dtu.dk/view_binary.php?type=data&mach=359


Developer: TMAH UV-lithography:<br /> http://labmanager.dtu.dk/view_binary.php?fileId=4434
Developer: TMAH UV-lithography:<br /> https://labmanager.dtu.dk/view_binary.php?type=data&mach=329


Spincoater: Süss stepper:<br /> http://labmanager.dtu.dk/view_binary.php?fileId=4433
Spincoater: Süss stepper:<br /> https://labmanager.dtu.dk/view_binary.php?type=data&mach=279


Developer: Stepper:<br /> http://labmanager.dtu.dk/view_binary.php?fileId=4435
Developer: Stepper:<br /> https://labmanager.dtu.dk/view_binary.php?type=data&mach=328


|


|
|
Line 222: Line 211:


= Hotplates =
= Hotplates =
'''Feedback to this section''': '''[mailto:labadviser@danchip.dtu.dk?Subject=Feed%20back%20from%20page%20http://labadviser.danchip.dtu.dk/index.php/Specific_Process_Knowledge/Lithography/Baking#Hotplates click here]'''


==Hotplate: 90-110C==   
==Hotplate: 90-110C==   
Line 228: Line 216:
Hotplate: 90-110C is used for baking of 2" - 6" wafers. Do not exceed 120°C.
Hotplate: 90-110C is used for baking of 2" - 6" wafers. Do not exceed 120°C.


'''The user manual, and contact information can be found in LabManager: [http://labmanager.danchip.dtu.dk/function.php?module=Machine&view=view&mach=336 Hotplate: 90-110C]'''
 
The user manual, and contact information can be found in LabManager:
 
[https://labmanager.dtu.dk/function.php?module=Machine&view=view&mach=336 Hotplate: 90-110C] - '''requires login'''


<br clear="all" />
<br clear="all" />


==Hotplate 1 (SU8), Hotplate 2 (SU8) and Hoplate 3(SU8)==
==SU-8 hotplates==
[[Image:SU-8hotplates.jpg|300x300px|thumb|Hotplate 1 (SU8) and Hotplate 2 (SU8) situated in C-1]]
[[Image:SU-8hotplates.jpg|300x300px|thumb|Hotplate 1 (SU8) and Hotplate 2 (SU8) (the old set-up in C-1)]]
We have three dedicated SU-8 hotplates in C-1 and E-4.
We have four hotplates dedicated to baking of SU-8.
<br>Hotplate 1 (SU8) and Hotplate 2 (SU8) are located in cleanroom E-4.
<br>Hotplate 3 (SU8) and Hotplate 4 (SU8) are located in PolyFabLab in building 347.


Users can control the ramp-time, the baking temperature, and the baking time.
Users can control the ramp-time, the baking temperature, and the baking time.
In order to avoid thermal curing of SU-8 residues on the hotplates, they are temperature limited to 110°C.
<br>The hotplates are temperature limited to 180°C.
 
 
The user manual, and contact information can be found in LabManager:
 
[https://labmanager.dtu.dk/function.php?module=Machine&view=view&mach=122 Hotplate 1 (SU8)] - '''requires login'''


'''The user manual, and contact information can be found in LabManager: [http://labmanager.danchip.dtu.dk/function.php?module=Machine&view=view&mach=122 Hotplate 1 (SU8)] [http://labmanager.danchip.dtu.dk/function.php?module=Machine&view=view&mach=124 Hotplate 2 (SU8)] [http://labmanager.danchip.dtu.dk/function.php?module=Machine&view=view&mach=453 Hotplate 3 (SU8)]'''
[https://labmanagerp.dtu.dk/function.php?module=Machine&view=view&mach=124 Hotplate 2 (SU8)] - '''requires login'''
 
[https://labmanager.dtu.dk/function.php?module=Machine&view=view&mach=453 Hotplate 3 (SU8)] - '''requires login'''
 
[https://labmanager.dtu.dk/function.php?module=Machine&view=view&mach=454 Hotplate 4 (SU8)] - '''requires login'''
<br clear="all" />
<br clear="all" />


Line 251: Line 253:
'''Actual surface temperature = 0.9 * display value'''
'''Actual surface temperature = 0.9 * display value'''


<div align="left">
<div align="right">
<gallery widths="320px" heights="240px">
<gallery widths="320px" heights="240px">
File:Benchtop C1.jpg|Benchtop hotplate for Spray coater located in C-1
File:Benchtop C1.jpg|Benchtop hotplate for Spray coater located in Cx1
File:Labspin_2.JPG|Benchtop hotplates for Labspins in E-5
File:Labspin_2.JPG|Benchtop hotplates for Labspins in E-5
</gallery>
</gallery>
Line 265: Line 267:


'''Information about the Süss MicroTec Gamma tools can be found in labadviser:'''  
'''Information about the Süss MicroTec Gamma tools can be found in labadviser:'''  
*[http://labadviser.danchip.dtu.dk/index.php/Specific_Process_Knowledge/Lithography/DUVStepperLithography#S.C3.9CSS_Spinner-Stepper Spin Coater: Süss Stepper]
*[https://labadviser.danchip.dtu.dk/index.php/Specific_Process_Knowledge/Lithography/Coaters#Spin_Coater:_Gamma_UV Spin Coater: Gamma UV]
*[http://labadviser.danchip.dtu.dk/index.php/Specific_Process_Knowledge/Lithography/DUVStepperLithography#Developer_TMAH_Stepper Developer: TMAH Stepper]
*[https://labadviser.danchip.dtu.dk/index.php/Specific_Process_Knowledge/Lithography/Coaters#Spin_Coater:_Gamma_E-beam_and_UV Spin Coater: Gamma e-beam & UV]
*[http://labadviser.danchip.dtu.dk/index.php/Specific_Process_Knowledge/Lithography/Development#Developer_TMAH_UV-lithography Developer TMAH UV-lithography]
*[https://labadviser.danchip.dtu.dk/index.php/Specific_Process_Knowledge/Lithography/Development#Developer_TMAH_UV-lithography Developer TMAH UV-lithography]
*[http://labadviser.danchip.dtu.dk/index.php/Specific_Process_Knowledge/Lithography/Coaters#Spin_Coater:_Gamma_UV Spin Coater: Gamma UV]
*[https://labadviser.danchip.dtu.dk/index.php/Specific_Process_Knowledge/Lithography/DUVStepperLithography#S.C3.9CSS_Spinner-Stepper Spin Coater: Süss Stepper]
*[http://labadviser.danchip.dtu.dk/index.php/Specific_Process_Knowledge/Lithography/Coaters#Spin_Coater:_Gamma_E-beam_and_UV Spin Coater: Gamma e-beam & UV]
*[https://labadviser.danchip.dtu.dk/index.php/Specific_Process_Knowledge/Lithography/DUVStepperLithography#Developer_TMAH_Stepper Developer: TMAH Stepper]


<br clear="all" />
<br clear="all" />


= Ovens =
= Ovens =
'''Feedback to this section''': '''[mailto:labadviser@danchip.dtu.dk?Subject=Feed%20back%20from%20page%20http://labadviser.danchip.dtu.dk/index.php/Specific_Process_Knowledge/Lithography/Baking#Ovens click here]'''
==Oven 90C==
[[Image:Oven_90_degrees_cr3.jpg|300x300px|thumb|Oven 90C situated in C-1]]
The oven is mostly used for baking of several wafers at a time at 90 °C as a soft baking step after a spin coating of photoresist. For 1.5µm resist the baking time is 30 min. For most of the other resist thicknesses it is also 30 min.
'''The user manual, and contact information can be found in LabManager: [http://labmanager.danchip.dtu.dk/function.php?module=Machine&view=view&mach=118 Oven 90C]'''
<br clear="all" />


==Oven: 110C - 250C==
==Oven: 110C - 250C==
Line 289: Line 283:
The set-point can be varied, but should always be returned to 110°C after use.
The set-point can be varied, but should always be returned to 110°C after use.


'''The user manual, and contact information can be found in LabManager: [http://labmanager.danchip.dtu.dk/function.php?module=Machine&view=view&mach=119 Oven: 110C - 250C]'''
 
The user manual, and contact information can be found in LabManager:
 
[https://labmanager.dtu.dk/function.php?module=Machine&view=view&mach=119 Oven: 110C - 250C] - '''requires login'''
<br clear="all" />
<br clear="all" />


==Oven 250C for pretreatment==
{{:Specific Process Knowledge/Lithography/Pretreatment/Oven_250C}}
[[Image:Oven_250_degrees_for_pretreatment_cr3.jpg|300x300px|thumb|Oven 250C for pretreatment situated in C-1]]
See [[Specific_Process_Knowledge/Lithography/Pretreatment#Oven_250C|'''Oven 250C''']]
<br clear="all" />

Latest revision as of 13:18, 31 July 2026

The content on this page, including all images and pictures, was created by DTU Nanolab staff, unless otherwise stated.

Feedback to this page: click here

Comparing baking methods

Spray coater hotplate SU-8 hotplates
(1 & 2 + 3 & 4)
Small benchtop hotplates Gamma hotplates Oven: 110C - 250C Oven 250C
Purpose

Adjustable temperature, contact bake

  • Soft bake
  • PEB
  • Hard bake

Programmable, ramped contact bake

  • Soft bake of SU-8
  • PEB of SU-8

Hotplate: 90-110C:
Programmable, contact bake

  • Soft bake
  • PEB


Labspin hotplates:
Adjustable temperature, contact bake

  • Soft bake
  • PEB
  • Hard bake

Recipe dependent temperature, contact or proximity bake

  • Soft bake
  • PEB
  • Hard bake

Manual convection bake

  • Hard bake
  • Post-exposure bake

Manual convection bake

  • Dehydration
  • NO resist!
Temperature

Maximum 180°C

Temperature with top-plate: Actual surface temperature = 0.9 * display value

Maximum 180°C

Hotplate: 90-110C:

  • Maximum 120°C
  • Return to 90°C after use


Labspin hotplates:

  • Maximum temperature is hotplate dependent
  • Temperature with top-plate: Actual surface temperature = 0.9 * display value

Fixed at various recipe dependent temperatures

110 - 250°C

Return to 110°C after use

Fixed at 250°C

Substrate size
  • Pieces
  • 50 mm wafer
  • 100 mm wafer
  • 150 mm wafer
  • 200 mm wafer
  • pieces
  • 50 mm wafers
  • 100 mm wafers
  • 150 mm wafer
  • 200 mm wafer
  • pieces (only Labspin hotplates)
  • 50 mm wafers
  • 100 mm wafers
  • 150 mm wafer
  • 200 mm wafer
  • 100 mm wafers
  • 150 mm wafers
  • 100 mm wafers
  • 150 mm wafers
  • 100 mm wafers
  • 150 mm wafers
Allowed materials

All substrates

Film or pattern of all types

Silicon, glass, and polymer substrates

Film or pattern of all types except type IV

Hotplate dependent.

(All substrates and film or pattern of all types, unless otherwise noted on the hotplate)

Tool dependent. Typically Silicon, III-V, and glass substrates.

Silicon, glass, and high Tg polymer substrates

Film or pattern of all types

Silicon, glass, and high Tg polymer substrates

Film or pattern of all types except resist

Restrictions
(Not allowed)
III-V, copper, steel substrates

Pb, Te films

Hotplate dependent. Any restrictions will be noted on the hotplate.

Low Tg polymer, copper, steel substrates.

Pb, Te films.

III-V, low Tg polymer, copper, steel substrates III-V, low Tg polymer, copper, steel substrates

Resist is not allowed

QC
- requires login

https://labmanager.dtu.dk/view_binary.php?type=data&mach=293

Hotplate 1:
https://labmanager.dtu.dk/view_binary.php?type=data&mach=122

Hotplate 2:
https://labmanager.dtu.dk/view_binary.php?type=data&mach=124


Hotplate: 90-110C:
https://labmanager.dtu.dk/view_binary.php?type=data&mach=336

Spin coater: Labspin 02:
https://labmanager.dtu.dk/view_binary.php?type=data&mach=362

Spin coater: Labspin 03:
https://labmanager.dtu.dk/view_binary.php?type=data&mach=387

Spincoater: Gamma ebeam & UV:
https://labmanager.dtu.dk/view_binary.php?type=data&mach=417

Spincoater: Gamma UV:
https://labmanager.dtu.dk/view_binary.php?type=data&mach=359

Developer: TMAH UV-lithography:
https://labmanager.dtu.dk/view_binary.php?type=data&mach=329

Spincoater: Süss stepper:
https://labmanager.dtu.dk/view_binary.php?type=data&mach=279

Developer: Stepper:
https://labmanager.dtu.dk/view_binary.php?type=data&mach=328




Hotplates

Hotplate: 90-110C

Hotplate: 90-110C located in C-1

Hotplate: 90-110C is used for baking of 2" - 6" wafers. Do not exceed 120°C.


The user manual, and contact information can be found in LabManager:

Hotplate: 90-110C - requires login


SU-8 hotplates

Hotplate 1 (SU8) and Hotplate 2 (SU8) (the old set-up in C-1)

We have four hotplates dedicated to baking of SU-8.
Hotplate 1 (SU8) and Hotplate 2 (SU8) are located in cleanroom E-4.
Hotplate 3 (SU8) and Hotplate 4 (SU8) are located in PolyFabLab in building 347.

Users can control the ramp-time, the baking temperature, and the baking time.
The hotplates are temperature limited to 180°C.


The user manual, and contact information can be found in LabManager:

Hotplate 1 (SU8) - requires login

Hotplate 2 (SU8) - requires login

Hotplate 3 (SU8) - requires login

Hotplate 4 (SU8) - requires login

Small benchtop hotplates

Model: Präzitherm PZ 28-2.

Contact bake only. Maximum temperature is hotplate dependent.

Most of these hotplates have been fitted with a top-plate in order to protect the original hotplate surface. With the top-plate, the set point of the controller must be adjusted in order to achieve the correct temperature during the bake:

Actual surface temperature = 0.9 * display value


Gamma hotplates

Hotplate modules in Spin Coater: Gamma UV.

Hotplate temperatures are recipe dependent.

Information about the Süss MicroTec Gamma tools can be found in labadviser:


Ovens

Oven: 110C - 250C

Oven: 110C - 250C situated in C-1

Variable temperature convection oven mostly used for baking of wafers as a hard baking step after development of photoresist.

The set-point can be varied, but should always be returned to 110°C after use.


The user manual, and contact information can be found in LabManager:

Oven: 110C - 250C - requires login

Oven 250C

Oven 250C for pretreatment in Cx-1

The oven is typically used for dehydration pretreatment, of Si and glass substrates, to promote the resist adhesion. We recommend placing the wafers in a metal carrier in the oven for at least for 4 hours, or overnight, and spin coat resist on them as soon as possible after removing them from the oven.


The user manual, and contact information can be found in LabManager:

Oven 250C - requires login