Jump to content

Specific Process Knowledge/Lithography/Baking: Difference between revisions

From LabAdviser
Jehem (talk | contribs)
Thes (talk | contribs)
No edit summary
 
(62 intermediate revisions by 3 users not shown)
Line 1: Line 1:
'''Feedback to this page''': '''[mailto:photolith@danchip.dtu.dk?Subject=Feed%20back%20from%20page%20http://labadviser.danchip.dtu.dk/index.php/Specific_Process_Knowledge/Lithography/Baking click here]'''
{{cc-nanolab}}
 
'''Feedback to this page''': '''[mailto:labadviser@nanolab.dtu.dk?Subject=Feed%20back%20from%20page%20https://labadviser.nanolab.dtu.dk/index.php?title=Specific_Process_Knowledge/Lithography/Baking click here]'''
 
[[Category: Equipment|baking]]
[[Category: Lithography|Baking]]
 
__TOC__


=Comparing baking methods=
=Comparing baking methods=


{|border="1" cellspacing="1" cellpadding="3" style="text-align:left;"  
{|border="1" cellspacing="1" cellpadding="10" style="text-align:left;"  
|-
|-


Line 9: Line 16:
|-style="background:silver; color:black"
|-style="background:silver; color:black"
!
!
![[Specific_Process_Knowledge/Lithography/Baking#Hotplate:_90-110C|Hotplate: 90-110C]]
![[Specific_Process_Knowledge/Lithography/Baking#Small benchtop hotplates|Spray coater hotplate]]
![[Specific_Process_Knowledge/Lithography/Baking#Hotplate_1_.28SU8.29.2C_Hotplate_2_.28SU8.29.2C_Hoplate_3.28SU8.29_and_Hotplate_4.28SU8.29|Hotplate 1, 2, 3 and 4(SU8)]]
![[Specific_Process_Knowledge/Lithography/Baking#SU-8 hotplates| SU-8 hotplates<br>(1 & 2 + 3 & 4)]]
![[Specific Process Knowledge/Lithography/Baking#Small_benchtop_hotplates|Small benchtop hotplates]]
![[Specific Process Knowledge/Lithography/Baking#Small_benchtop_hotplates|Small benchtop hotplates]]
![[Specific Process Knowledge/Lithography/Baking#Gamma_hotplates|Gamma hotplates]]
![[Specific Process Knowledge/Lithography/Baking#Gamma_hotplates|Gamma hotplates]]
![[Specific_Process_Knowledge/Lithography/Baking#Oven 90C|Oven 90C]]
![[Specific_Process_Knowledge/Lithography/Baking#Oven: 110C - 250C|Oven: 110C - 250C]]
![[Specific_Process_Knowledge/Lithography/Baking#Oven: 110C - 250C|Oven: 110C - 250C]]
![[Specific Process Knowledge/Lithography/Pretreatment#Oven 250C|Oven 250C]]
![[Specific Process Knowledge/Lithography/Baking#Oven_250C|Oven 250C]]
|-
|-


Line 22: Line 28:
!Purpose
!Purpose
|
|
Programmable, contact bake
Adjustable temperature, contact bake
*Soft bake
*Soft bake
*PEB
*PEB
*Hard bake
|
|
Programmable, ramped contact bake
Programmable, ramped contact bake
Line 30: Line 37:
*PEB of SU-8
*PEB of SU-8
|
|
Hotplate: 90-110C:<br />
Programmable, contact bake
*Soft bake
*PEB
Labspin hotplates:<br />
Adjustable temperature, contact bake
Adjustable temperature, contact bake
*Soft bake
*Soft bake
Line 39: Line 53:
*PEB
*PEB
*Hard bake
*Hard bake
|
Manual convection bake
*Soft bake
|
|
Manual convection bake
Manual convection bake
Line 56: Line 67:
!Temperature
!Temperature
|
|
Maximum 120°C
Maximum 180°C
 
Temperature with top-plate: Actual surface temperature = 0.9 * display value
|
|
Maximum 110°C
Maximum 180°C
|
|
Maximum temperature is hotplate dependent
Hotplate: 90-110C:<br />
*Maximum 120°C
*Return to 90°C after use
 
 
Labspin hotplates:<br />
*Maximum temperature is hotplate dependent
*Temperature with top-plate: Actual surface temperature = 0.9 * display value
|
|
Fixed at various recipe dependent temperatures.
Fixed at various recipe dependent temperatures
|
Fixed at 90°C
|
|
110 - 250°C
110 - 250°C
Line 77: Line 95:
!Substrate size
!Substrate size
|
|
* Pieces
* 50 mm wafer
* 50 mm wafer
* 100 mm wafer
* 100 mm wafer
* 150 mm wafer
* 150 mm wafer
* 200 mm wafer
|
|
* pieces
* pieces
Line 87: Line 107:
* 200 mm wafer
* 200 mm wafer
|
|
* pieces
* pieces (only Labspin hotplates)
* 50 mm wafers
* 50 mm wafers
* 100 mm wafers
* 100 mm wafers
* 150 mm wafer
* 150 mm wafer
* 200 mm wafer
* 200 mm wafer
|
* 100 mm wafers
* 150 mm wafers
|
|
* 100 mm wafers
* 100 mm wafers
Line 121: Line 138:
(All substrates and film or pattern of all types, unless otherwise noted on the hotplate)
(All substrates and film or pattern of all types, unless otherwise noted on the hotplate)
|
|
Silicon and glass substrates
Tool dependent. Typically Silicon, III-V, and glass substrates.
|
Silicon, glass, and polymer substrates
 
Film or pattern of all types
|
|
Silicon, glass, and high Tg polymer substrates
Silicon, glass, and high Tg polymer substrates
Line 133: Line 146:
Silicon, glass, and high Tg polymer substrates
Silicon, glass, and high Tg polymer substrates


Film or pattern of all types except resist|
Film or pattern of all types except resist
|-
|-


Line 146: Line 159:
Hotplate dependent. Any restrictions will be noted on the hotplate.
Hotplate dependent. Any restrictions will be noted on the hotplate.
|
|
Low Tg polymer, copper, steel substrates.


|III-V, copper, steel substrates
Pb, Te films.
|III-V, low Tg polymer, copper, steel substrates
|III-V, low Tg polymer, copper, steel substrates
|III-V, low Tg polymer, copper, steel substrates
|III-V, low Tg polymer, copper, steel substrates
Line 155: Line 169:




|-style="background:WhiteSmoke; color:black"
|-style="background:WhiteSmoke; color:black"
!QC
|- valign="top"
!QC<br>'''- requires login'''
|
|
Comming soon.
https://labmanager.dtu.dk/view_binary.php?type=data&mach=293
 
|
|
Comming soon.
Hotplate 1:<br /> https://labmanager.dtu.dk/view_binary.php?type=data&mach=122
|
Comming soon.
|
'''Spincoater: Gamma UV:'''


* TM16 @ 110°C: Mean 110.1°C, uniformity error 0.23%.
Hotplate 2:<br /> https://labmanager.dtu.dk/view_binary.php?type=data&mach=124
* TM15 @ 100°C: Mean 99.5°C, uniformity error 0.95%.
* TM14 @ 90°C: Mean 88.9°C, uniformity error 1.01%.
* TM13 @ 110°C: Mean 108.6°C, uniformity error 1.45%.


|
Hotplate: 90-110C:<br /> https://labmanager.dtu.dk/view_binary.php?type=data&mach=336


'''Developer: TMAH UV-lithography:'''
Spin coater: Labspin 02:<br />https://labmanager.dtu.dk/view_binary.php?type=data&mach=362


Coming soon.
Spin coater: Labspin 03:<br />https://labmanager.dtu.dk/view_binary.php?type=data&mach=387


|
Spincoater: Gamma ebeam & UV:<br />  https://labmanager.dtu.dk/view_binary.php?type=data&mach=417


'''Spincoater: Süss stepper:'''
Spincoater: Gamma UV:<br />  https://labmanager.dtu.dk/view_binary.php?type=data&mach=359
 
* TM16 @ 175°C: Mean 174.4°C, uniformity error 0.72%.
* TM15 @ 175C: Mean 174.9°C, uniformity error 0.15%.
* TM14 @ 130°C: Mean 129.8°C, uniformity error 0.23%.
* TM13 @ 130°C: Mean 129.7°C, uniformity error 0.20%.
* TM12 @ 23°C: Mean 22.9°C, uniformity error 0.46%.
* TM11 @ 23°C: Mean 22.8°C, uniformity error 0.46%.
 


'''Developer: Stepper:'''
Developer: TMAH UV-lithography:<br /> https://labmanager.dtu.dk/view_binary.php?type=data&mach=329


* TM14 @ 130°C: Mean 129.9°C, uniformity error 0.62%.
Spincoater: Süss stepper:<br /> https://labmanager.dtu.dk/view_binary.php?type=data&mach=279
* TM13 @ 130°C: Mean 130.1°C, uniformity error 0.73%.
* TM11 @ 20°C: Mean 20.2°C, uniformity error 0.10%.


Developer: Stepper:<br /> https://labmanager.dtu.dk/view_binary.php?type=data&mach=328


|


|
|
Line 207: Line 211:


= Hotplates =
= Hotplates =
'''Feedback to this section''': '''[mailto:labadviser@danchip.dtu.dk?Subject=Feed%20back%20from%20page%20http://labadviser.danchip.dtu.dk/index.php/Specific_Process_Knowledge/Lithography/Baking#Hotplates click here]'''


==Hotplate: 90-110C==   
==Hotplate: 90-110C==   
Line 213: Line 216:
Hotplate: 90-110C is used for baking of 2" - 6" wafers. Do not exceed 120°C.
Hotplate: 90-110C is used for baking of 2" - 6" wafers. Do not exceed 120°C.


'''The user manual, and contact information can be found in LabManager: [http://labmanager.danchip.dtu.dk/function.php?module=Machine&view=view&mach=336 Hotplate: 90-110C]'''
 
The user manual, and contact information can be found in LabManager:
 
[https://labmanager.dtu.dk/function.php?module=Machine&view=view&mach=336 Hotplate: 90-110C] - '''requires login'''


<br clear="all" />
<br clear="all" />


==Hotplate 1 (SU8), Hotplate 2 (SU8), Hoplate 3(SU8) and Hotplate 4(SU8)==
==SU-8 hotplates==
[[Image:SU-8hotplates.jpg|300x300px|thumb|Hotplate 1 (SU8) and Hotplate 2 (SU8) situated in C-1]]
[[Image:SU-8hotplates.jpg|300x300px|thumb|Hotplate 1 (SU8) and Hotplate 2 (SU8) (the old set-up in C-1)]]
We have four dedicated SU-8 hotplates in C-1.
We have four hotplates dedicated to baking of SU-8.
<br>Hotplate 1 (SU8) and Hotplate 2 (SU8) are located in cleanroom E-4.
<br>Hotplate 3 (SU8) and Hotplate 4 (SU8) are located in PolyFabLab in building 347.


Users can control the ramp-time, the baking temperature, and the baking time.
Users can control the ramp-time, the baking temperature, and the baking time.
In order to avoid thermal curing of SU-8 residues on the hotplates, they are temperature limited to 110°C.
<br>The hotplates are temperature limited to 180°C.
 
 
The user manual, and contact information can be found in LabManager:
 
[https://labmanager.dtu.dk/function.php?module=Machine&view=view&mach=122 Hotplate 1 (SU8)] - '''requires login'''


'''The user manual, and contact information can be found in LabManager: [http://labmanager.danchip.dtu.dk/function.php?module=Machine&view=view&mach=122 Hotplate 1 (SU8)] [http://labmanager.danchip.dtu.dk/function.php?module=Machine&view=view&mach=124 Hotplate 2 (SU8)] [http://labmanager.danchip.dtu.dk/function.php?module=Machine&view=view&mach=543 Hotplate 3 (SU8)] [http://labmanager.danchip.dtu.dk/function.php?module=Machine&view=view&mach=454 Hotplate 4 (SU8)]'''
[https://labmanagerp.dtu.dk/function.php?module=Machine&view=view&mach=124 Hotplate 2 (SU8)] - '''requires login'''
 
[https://labmanager.dtu.dk/function.php?module=Machine&view=view&mach=453 Hotplate 3 (SU8)] - '''requires login'''
 
[https://labmanager.dtu.dk/function.php?module=Machine&view=view&mach=454 Hotplate 4 (SU8)] - '''requires login'''
<br clear="all" />
<br clear="all" />


Line 232: Line 249:
Contact bake only. Maximum temperature is hotplate dependent.
Contact bake only. Maximum temperature is hotplate dependent.


<div align="left">
Most of these hotplates have been fitted with a top-plate in order to protect the original hotplate surface. With the top-plate, the set point of the controller must be adjusted in order to achieve the correct temperature during the bake:
<gallery widths="200px" heights="150px">
 
File:Benchtop A5 1.jpg|Benchtop hotplate located in A-5
'''Actual surface temperature = 0.9 * display value'''
File:Benchtop A5 2.jpg|Benchtop hotplates located in A-5
 
File:Benchtop C1.jpg|Benchtop hotplate located in C-1
<div align="right">
File:Benchtop E5.jpg|Benchtop hotplate located in E-5
<gallery widths="320px" heights="240px">
File:Benchtop C1.jpg|Benchtop hotplate for Spray coater located in Cx1
File:Labspin_2.JPG|Benchtop hotplates for Labspins in E-5
</gallery>
</gallery>
</div>
</div>
Line 244: Line 263:


==Gamma hotplates==   
==Gamma hotplates==   
[[Image:HMDS gammaUV.jpg|300x300px|thumb|Hotplate modules in Gamma UV spincoater.]]
[[Image:HMDS gammaUV.jpg|300x300px|thumb|Hotplate modules in Spin Coater: Gamma UV.]]
Hotplate temperatures are recipe dependent.
Hotplate temperatures are recipe dependent.


'''Information about the Süss MicroTec Gamma tools can be found in labadviser:'''  
'''Information about the Süss MicroTec Gamma tools can be found in labadviser:'''  
*[http://labadviser.danchip.dtu.dk/index.php/Specific_Process_Knowledge/Lithography/DUVStepperLithography#S.C3.9CSS_Spinner-Stepper Spin Coater: Süss Stepper]
*[https://labadviser.danchip.dtu.dk/index.php/Specific_Process_Knowledge/Lithography/Coaters#Spin_Coater:_Gamma_UV Spin Coater: Gamma UV]
*[http://labadviser.danchip.dtu.dk/index.php/Specific_Process_Knowledge/Lithography/DUVStepperLithography#Developer_TMAH_Stepper Developer: TMAH Stepper]
*[https://labadviser.danchip.dtu.dk/index.php/Specific_Process_Knowledge/Lithography/Coaters#Spin_Coater:_Gamma_E-beam_and_UV Spin Coater: Gamma e-beam & UV]
*[http://labadviser.danchip.dtu.dk/index.php/Specific_Process_Knowledge/Lithography/Development#Developer_TMAH_UV-lithography Developer TMAH UV-lithography]
*[https://labadviser.danchip.dtu.dk/index.php/Specific_Process_Knowledge/Lithography/Development#Developer_TMAH_UV-lithography Developer TMAH UV-lithography]
*[http://labadviser.danchip.dtu.dk/index.php/Specific_Process_Knowledge/Lithography/Coaters#Spin_Coater:_Gamma_UV Spin Coater: Gamma UV]
*[https://labadviser.danchip.dtu.dk/index.php/Specific_Process_Knowledge/Lithography/DUVStepperLithography#S.C3.9CSS_Spinner-Stepper Spin Coater: Süss Stepper]
*[http://labadviser.danchip.dtu.dk/index.php/Specific_Process_Knowledge/Lithography/Coaters#Spin_Coater:_Gamma_E-beam_and_UV Spin Coater: Gamma e-beam & UV]
*[https://labadviser.danchip.dtu.dk/index.php/Specific_Process_Knowledge/Lithography/DUVStepperLithography#Developer_TMAH_Stepper Developer: TMAH Stepper]


<br clear="all" />
<br clear="all" />


= Ovens =
= Ovens =
'''Feedback to this section''': '''[mailto:labadviser@danchip.dtu.dk?Subject=Feed%20back%20from%20page%20http://labadviser.danchip.dtu.dk/index.php/Specific_Process_Knowledge/Lithography/Baking#Ovens click here]'''
==Oven 90C==
[[Image:Oven_90_degrees_cr3.jpg|300x300px|thumb|Oven 90C situated in C-1]]
The oven is mostly used for baking of several wafers at a time at 90 °C as a soft baking step after a spin coating of photoresist. For 1.5µm resist the baking time is 30 min. For most of the other resist thicknesses it is also 30 min.
'''The user manual, and contact information can be found in LabManager: [http://labmanager.danchip.dtu.dk/function.php?module=Machine&view=view&mach=118 Oven 90C]'''
<br clear="all" />


==Oven: 110C - 250C==
==Oven: 110C - 250C==
Line 272: Line 283:
The set-point can be varied, but should always be returned to 110°C after use.
The set-point can be varied, but should always be returned to 110°C after use.


'''The user manual, and contact information can be found in LabManager: [http://labmanager.danchip.dtu.dk/function.php?module=Machine&view=view&mach=119 Oven: 110C - 250C]'''
 
The user manual, and contact information can be found in LabManager:
 
[https://labmanager.dtu.dk/function.php?module=Machine&view=view&mach=119 Oven: 110C - 250C] - '''requires login'''
<br clear="all" />
<br clear="all" />


==Oven 250C for pretreatment==
{{:Specific Process Knowledge/Lithography/Pretreatment/Oven_250C}}
[[Image:Oven_250_degrees_for_pretreatment_cr3.jpg|300x300px|thumb|Oven 250C for pretreatment situated in C-1]]
See [[Specific_Process_Knowledge/Lithography/Pretreatment#Oven_250C|'''Oven 250C''']]
<br clear="all" />

Latest revision as of 13:18, 31 July 2026

The content on this page, including all images and pictures, was created by DTU Nanolab staff, unless otherwise stated.

Feedback to this page: click here

Comparing baking methods

Spray coater hotplate SU-8 hotplates
(1 & 2 + 3 & 4)
Small benchtop hotplates Gamma hotplates Oven: 110C - 250C Oven 250C
Purpose

Adjustable temperature, contact bake

  • Soft bake
  • PEB
  • Hard bake

Programmable, ramped contact bake

  • Soft bake of SU-8
  • PEB of SU-8

Hotplate: 90-110C:
Programmable, contact bake

  • Soft bake
  • PEB


Labspin hotplates:
Adjustable temperature, contact bake

  • Soft bake
  • PEB
  • Hard bake

Recipe dependent temperature, contact or proximity bake

  • Soft bake
  • PEB
  • Hard bake

Manual convection bake

  • Hard bake
  • Post-exposure bake

Manual convection bake

  • Dehydration
  • NO resist!
Temperature

Maximum 180°C

Temperature with top-plate: Actual surface temperature = 0.9 * display value

Maximum 180°C

Hotplate: 90-110C:

  • Maximum 120°C
  • Return to 90°C after use


Labspin hotplates:

  • Maximum temperature is hotplate dependent
  • Temperature with top-plate: Actual surface temperature = 0.9 * display value

Fixed at various recipe dependent temperatures

110 - 250°C

Return to 110°C after use

Fixed at 250°C

Substrate size
  • Pieces
  • 50 mm wafer
  • 100 mm wafer
  • 150 mm wafer
  • 200 mm wafer
  • pieces
  • 50 mm wafers
  • 100 mm wafers
  • 150 mm wafer
  • 200 mm wafer
  • pieces (only Labspin hotplates)
  • 50 mm wafers
  • 100 mm wafers
  • 150 mm wafer
  • 200 mm wafer
  • 100 mm wafers
  • 150 mm wafers
  • 100 mm wafers
  • 150 mm wafers
  • 100 mm wafers
  • 150 mm wafers
Allowed materials

All substrates

Film or pattern of all types

Silicon, glass, and polymer substrates

Film or pattern of all types except type IV

Hotplate dependent.

(All substrates and film or pattern of all types, unless otherwise noted on the hotplate)

Tool dependent. Typically Silicon, III-V, and glass substrates.

Silicon, glass, and high Tg polymer substrates

Film or pattern of all types

Silicon, glass, and high Tg polymer substrates

Film or pattern of all types except resist

Restrictions
(Not allowed)
III-V, copper, steel substrates

Pb, Te films

Hotplate dependent. Any restrictions will be noted on the hotplate.

Low Tg polymer, copper, steel substrates.

Pb, Te films.

III-V, low Tg polymer, copper, steel substrates III-V, low Tg polymer, copper, steel substrates

Resist is not allowed

QC
- requires login

https://labmanager.dtu.dk/view_binary.php?type=data&mach=293

Hotplate 1:
https://labmanager.dtu.dk/view_binary.php?type=data&mach=122

Hotplate 2:
https://labmanager.dtu.dk/view_binary.php?type=data&mach=124


Hotplate: 90-110C:
https://labmanager.dtu.dk/view_binary.php?type=data&mach=336

Spin coater: Labspin 02:
https://labmanager.dtu.dk/view_binary.php?type=data&mach=362

Spin coater: Labspin 03:
https://labmanager.dtu.dk/view_binary.php?type=data&mach=387

Spincoater: Gamma ebeam & UV:
https://labmanager.dtu.dk/view_binary.php?type=data&mach=417

Spincoater: Gamma UV:
https://labmanager.dtu.dk/view_binary.php?type=data&mach=359

Developer: TMAH UV-lithography:
https://labmanager.dtu.dk/view_binary.php?type=data&mach=329

Spincoater: Süss stepper:
https://labmanager.dtu.dk/view_binary.php?type=data&mach=279

Developer: Stepper:
https://labmanager.dtu.dk/view_binary.php?type=data&mach=328




Hotplates

Hotplate: 90-110C

Hotplate: 90-110C located in C-1

Hotplate: 90-110C is used for baking of 2" - 6" wafers. Do not exceed 120°C.


The user manual, and contact information can be found in LabManager:

Hotplate: 90-110C - requires login


SU-8 hotplates

Hotplate 1 (SU8) and Hotplate 2 (SU8) (the old set-up in C-1)

We have four hotplates dedicated to baking of SU-8.
Hotplate 1 (SU8) and Hotplate 2 (SU8) are located in cleanroom E-4.
Hotplate 3 (SU8) and Hotplate 4 (SU8) are located in PolyFabLab in building 347.

Users can control the ramp-time, the baking temperature, and the baking time.
The hotplates are temperature limited to 180°C.


The user manual, and contact information can be found in LabManager:

Hotplate 1 (SU8) - requires login

Hotplate 2 (SU8) - requires login

Hotplate 3 (SU8) - requires login

Hotplate 4 (SU8) - requires login

Small benchtop hotplates

Model: Präzitherm PZ 28-2.

Contact bake only. Maximum temperature is hotplate dependent.

Most of these hotplates have been fitted with a top-plate in order to protect the original hotplate surface. With the top-plate, the set point of the controller must be adjusted in order to achieve the correct temperature during the bake:

Actual surface temperature = 0.9 * display value


Gamma hotplates

Hotplate modules in Spin Coater: Gamma UV.

Hotplate temperatures are recipe dependent.

Information about the Süss MicroTec Gamma tools can be found in labadviser:


Ovens

Oven: 110C - 250C

Oven: 110C - 250C situated in C-1

Variable temperature convection oven mostly used for baking of wafers as a hard baking step after development of photoresist.

The set-point can be varied, but should always be returned to 110°C after use.


The user manual, and contact information can be found in LabManager:

Oven: 110C - 250C - requires login

Oven 250C

Oven 250C for pretreatment in Cx-1

The oven is typically used for dehydration pretreatment, of Si and glass substrates, to promote the resist adhesion. We recommend placing the wafers in a metal carrier in the oven for at least for 4 hours, or overnight, and spin coat resist on them as soon as possible after removing them from the oven.