Specific Process Knowledge/Lithography/Baking: Difference between revisions
No edit summary |
|||
| (138 intermediate revisions by 5 users not shown) | |||
| Line 1: | Line 1: | ||
'''Feedback to this page''': '''[mailto: | {{cc-nanolab}} | ||
'''Feedback to this page''': '''[mailto:labadviser@nanolab.dtu.dk?Subject=Feed%20back%20from%20page%20https://labadviser.nanolab.dtu.dk/index.php?title=Specific_Process_Knowledge/Lithography/Baking click here]''' | |||
[[Category: Equipment|baking]] | |||
[[Category: Lithography|Baking]] | |||
__TOC__ | |||
=Comparing baking methods= | =Comparing baking methods= | ||
{|border="1" cellspacing="1" cellpadding=" | {|border="1" cellspacing="1" cellpadding="10" style="text-align:left;" | ||
|- | |- | ||
| Line 9: | Line 16: | ||
|-style="background:silver; color:black" | |-style="background:silver; color:black" | ||
! | ! | ||
![[Specific_Process_Knowledge/Lithography/Baking# | ![[Specific_Process_Knowledge/Lithography/Baking#Small benchtop hotplates|Spray coater hotplate]] | ||
![[Specific_Process_Knowledge/Lithography/Baking# | ![[Specific_Process_Knowledge/Lithography/Baking#SU-8 hotplates| SU-8 hotplates<br>(1 & 2 + 3 & 4)]] | ||
![[Specific Process Knowledge/Lithography/Baking#Small_benchtop_hotplates|Small benchtop hotplates]] | ![[Specific Process Knowledge/Lithography/Baking#Small_benchtop_hotplates|Small benchtop hotplates]] | ||
![[Specific Process Knowledge/Lithography/Baking#Gamma_hotplates|Gamma hotplates]] | ![[Specific Process Knowledge/Lithography/Baking#Gamma_hotplates|Gamma hotplates]] | ||
![[Specific_Process_Knowledge/Lithography/Baking#Oven: 110C - 250C|Oven: 110C - 250C]] | ![[Specific_Process_Knowledge/Lithography/Baking#Oven: 110C - 250C|Oven: 110C - 250C]] | ||
![[Specific Process Knowledge/Lithography/ | ![[Specific Process Knowledge/Lithography/Baking#Oven_250C|Oven 250C]] | ||
|- | |- | ||
| Line 22: | Line 28: | ||
!Purpose | !Purpose | ||
| | | | ||
Adjustable temperature, contact bake | |||
*Soft bake | *Soft bake | ||
*PEB | *PEB | ||
*Hard bake | |||
| | | | ||
Programmable, ramped contact bake | Programmable, ramped contact bake | ||
| Line 30: | Line 37: | ||
*PEB of SU-8 | *PEB of SU-8 | ||
| | | | ||
Hotplate: 90-110C:<br /> | |||
Programmable, contact bake | |||
*Soft bake | |||
*PEB | |||
Labspin hotplates:<br /> | |||
Adjustable temperature, contact bake | |||
*Soft bake | |||
*PEB | |||
*Hard bake | |||
| | | | ||
Recipe dependent temperature, contact or proximity bake | |||
*Soft bake | *Soft bake | ||
*PEB | |||
*Hard bake | |||
| | | | ||
Manual convection bake | Manual convection bake | ||
| Line 43: | Line 60: | ||
Manual convection bake | Manual convection bake | ||
*Dehydration | *Dehydration | ||
*'''NO resist!''' | |||
|- | |- | ||
| Line 49: | Line 67: | ||
!Temperature | !Temperature | ||
| | | | ||
Maximum | Maximum 180°C | ||
Temperature with top-plate: Actual surface temperature = 0.9 * display value | |||
| | | | ||
Maximum 180°C | |||
| | | | ||
Hotplate: 90-110C:<br /> | |||
*Maximum 120°C | |||
*Return to 90°C after use | |||
Labspin hotplates:<br /> | |||
*Maximum temperature is hotplate dependent | |||
*Temperature with top-plate: Actual surface temperature = 0.9 * display value | |||
| | | | ||
Fixed at | Fixed at various recipe dependent temperatures | ||
| | | | ||
110 - 250°C | 110 - 250°C | ||
| Line 68: | Line 95: | ||
!Substrate size | !Substrate size | ||
| | | | ||
* Pieces | |||
* 50 mm wafer | * 50 mm wafer | ||
* 100 mm wafer | * 100 mm wafer | ||
* 150 mm wafer | * 150 mm wafer | ||
* 200 mm wafer | |||
| | | | ||
* pieces | * pieces | ||
| Line 78: | Line 107: | ||
* 200 mm wafer | * 200 mm wafer | ||
| | | | ||
* pieces (only Labspin hotplates) | |||
* 50 mm wafers | |||
* 100 mm wafers | |||
* 150 mm wafer | |||
* 200 mm wafer | |||
| | | | ||
* 100 mm wafers | * 100 mm wafers | ||
| Line 101: | Line 134: | ||
Film or pattern of all types except type IV | Film or pattern of all types except type IV | ||
| | | | ||
Hotplate dependent. | |||
(All substrates and film or pattern of all types, unless otherwise noted on the hotplate) | |||
| | | | ||
Tool dependent. Typically Silicon, III-V, and glass substrates. | |||
Silicon, | |||
| | | | ||
Silicon, glass, and high Tg polymer substrates | Silicon, glass, and high Tg polymer substrates | ||
| Line 113: | Line 146: | ||
Silicon, glass, and high Tg polymer substrates | Silicon, glass, and high Tg polymer substrates | ||
Film or pattern of all types except resist | Film or pattern of all types except resist | ||
|- | |- | ||
| Line 124: | Line 157: | ||
Pb, Te films | Pb, Te films | ||
| | | | ||
Hotplate dependent. Any restrictions will be noted on the hotplate. | |||
| | | | ||
Low Tg polymer, copper, steel substrates. | |||
Pb, Te films. | |||
|III-V, low Tg polymer, copper, steel substrates | |III-V, low Tg polymer, copper, steel substrates | ||
|III-V, low Tg polymer, copper, steel substrates | |III-V, low Tg polymer, copper, steel substrates | ||
| Line 134: | Line 169: | ||
|-style="background:WhiteSmoke; color:black" | |-style="background:WhiteSmoke; color:black" | ||
!QC | |- valign="top" | ||
!QC<br>'''- requires login''' | |||
| | | | ||
https://labmanager.dtu.dk/view_binary.php?type=data&mach=293 | |||
| | | | ||
Hotplate 1:<br /> https://labmanager.dtu.dk/view_binary.php?type=data&mach=122 | |||
Hotplate 2:<br /> https://labmanager.dtu.dk/view_binary.php?type=data&mach=124 | |||
| | | | ||
Hotplate: 90-110C:<br /> https://labmanager.dtu.dk/view_binary.php?type=data&mach=336 | |||
Spin coater: Labspin 02:<br />https://labmanager.dtu.dk/view_binary.php?type=data&mach=362 | |||
Spin coater: Labspin 03:<br />https://labmanager.dtu.dk/view_binary.php?type=data&mach=387 | |||
| | | | ||
Spincoater: Gamma ebeam & UV:<br /> https://labmanager.dtu.dk/view_binary.php?type=data&mach=417 | |||
Spincoater: Gamma UV:<br /> https://labmanager.dtu.dk/view_binary.php?type=data&mach=359 | |||
Developer: TMAH UV-lithography:<br /> https://labmanager.dtu.dk/view_binary.php?type=data&mach=329 | |||
Spincoater: Süss stepper:<br /> https://labmanager.dtu.dk/view_binary.php?type=data&mach=279 | |||
Developer: Stepper:<br /> https://labmanager.dtu.dk/view_binary.php?type=data&mach=328 | |||
| | | | ||
| | | | ||
|- | |- | ||
|} | |} | ||
| Line 157: | Line 211: | ||
= Hotplates = | = Hotplates = | ||
==Hotplate: 90-110C== | ==Hotplate: 90-110C== | ||
[[Image:Hotplate90-110C in C-1.jpg|300x300px|thumb| | [[Image:Hotplate90-110C in C-1.jpg|300x300px|thumb|Hotplate: 90-110C located in C-1]] | ||
Hotplate: 90-110C is used for baking of 2" - 6" wafers. Do not exceed 120°C. | Hotplate: 90-110C is used for baking of 2" - 6" wafers. Do not exceed 120°C. | ||
The user manual, and contact information can be found in LabManager: | |||
[https://labmanager.dtu.dk/function.php?module=Machine&view=view&mach=336 Hotplate: 90-110C] - '''requires login''' | |||
<br clear="all" /> | <br clear="all" /> | ||
== | ==SU-8 hotplates== | ||
[[Image:SU-8hotplates.jpg|300x300px|thumb|Hotplate 1 (SU8) and Hotplate 2 (SU8) | [[Image:SU-8hotplates.jpg|300x300px|thumb|Hotplate 1 (SU8) and Hotplate 2 (SU8) (the old set-up in C-1)]] | ||
We have | We have four hotplates dedicated to baking of SU-8. | ||
<br>Hotplate 1 (SU8) and Hotplate 2 (SU8) are located in cleanroom E-4. | |||
<br>Hotplate 3 (SU8) and Hotplate 4 (SU8) are located in PolyFabLab in building 347. | |||
Users can control the ramp-time, the baking temperature, and the baking time. | Users can control the ramp-time, the baking temperature, and the baking time. | ||
<br>The hotplates are temperature limited to 180°C. | |||
The user manual, and contact information can be found in LabManager: | |||
[https://labmanager.dtu.dk/function.php?module=Machine&view=view&mach=122 Hotplate 1 (SU8)] - '''requires login''' | |||
[https://labmanagerp.dtu.dk/function.php?module=Machine&view=view&mach=124 Hotplate 2 (SU8)] - '''requires login''' | |||
[https://labmanager.dtu.dk/function.php?module=Machine&view=view&mach=453 Hotplate 3 (SU8)] - '''requires login''' | |||
[https://labmanager.dtu.dk/function.php?module=Machine&view=view&mach=454 Hotplate 4 (SU8)] - '''requires login''' | |||
<br clear="all" /> | <br clear="all" /> | ||
==Small benchtop hotplates== | ==Small benchtop hotplates== | ||
Model: Präzitherm PZ 28-2. | |||
Contact bake only. Maximum temperature is hotplate dependent. | |||
Most of these hotplates have been fitted with a top-plate in order to protect the original hotplate surface. With the top-plate, the set point of the controller must be adjusted in order to achieve the correct temperature during the bake: | |||
'''Actual surface temperature = 0.9 * display value''' | |||
<div align="right"> | |||
<gallery widths="320px" heights="240px"> | |||
File:Benchtop C1.jpg|Benchtop hotplate for Spray coater located in Cx1 | |||
File:Labspin_2.JPG|Benchtop hotplates for Labspins in E-5 | |||
</gallery> | |||
</div> | |||
<br clear="all" /> | <br clear="all" /> | ||
==Gamma hotplates== | ==Gamma hotplates== | ||
[[Image:HMDS gammaUV.jpg|300x300px|thumb|Hotplate modules in Spin Coater: Gamma UV.]] | |||
Hotplate temperatures are recipe dependent. | |||
'''Information about the Süss MicroTec Gamma tools can be found in labadviser:''' | |||
*[https://labadviser.danchip.dtu.dk/index.php/Specific_Process_Knowledge/Lithography/Coaters#Spin_Coater:_Gamma_UV Spin Coater: Gamma UV] | |||
*[https://labadviser.danchip.dtu.dk/index.php/Specific_Process_Knowledge/Lithography/Coaters#Spin_Coater:_Gamma_E-beam_and_UV Spin Coater: Gamma e-beam & UV] | |||
*[https://labadviser.danchip.dtu.dk/index.php/Specific_Process_Knowledge/Lithography/Development#Developer_TMAH_UV-lithography Developer TMAH UV-lithography] | |||
*[https://labadviser.danchip.dtu.dk/index.php/Specific_Process_Knowledge/Lithography/DUVStepperLithography#S.C3.9CSS_Spinner-Stepper Spin Coater: Süss Stepper] | |||
*[https://labadviser.danchip.dtu.dk/index.php/Specific_Process_Knowledge/Lithography/DUVStepperLithography#Developer_TMAH_Stepper Developer: TMAH Stepper] | |||
<br clear="all" /> | <br clear="all" /> | ||
= Ovens = | = Ovens = | ||
==Oven: 110C - 250C== | ==Oven: 110C - 250C== | ||
| Line 203: | Line 283: | ||
The set-point can be varied, but should always be returned to 110°C after use. | The set-point can be varied, but should always be returned to 110°C after use. | ||
The user manual, and contact information can be found in LabManager: | |||
[https://labmanager.dtu.dk/function.php?module=Machine&view=view&mach=119 Oven: 110C - 250C] - '''requires login''' | |||
<br clear="all" /> | <br clear="all" /> | ||
{{:Specific Process Knowledge/Lithography/Pretreatment/Oven_250C}} | |||
Latest revision as of 13:18, 31 July 2026
The content on this page, including all images and pictures, was created by DTU Nanolab staff, unless otherwise stated.
Feedback to this page: click here
Comparing baking methods
| Spray coater hotplate | SU-8 hotplates (1 & 2 + 3 & 4) |
Small benchtop hotplates | Gamma hotplates | Oven: 110C - 250C | Oven 250C | |
|---|---|---|---|---|---|---|
| Purpose |
Adjustable temperature, contact bake
|
Programmable, ramped contact bake
|
Hotplate: 90-110C:
|
Recipe dependent temperature, contact or proximity bake
|
Manual convection bake
|
Manual convection bake
|
| Temperature |
Maximum 180°C Temperature with top-plate: Actual surface temperature = 0.9 * display value |
Maximum 180°C |
Hotplate: 90-110C:
|
Fixed at various recipe dependent temperatures |
110 - 250°C Return to 110°C after use |
Fixed at 250°C |
| Substrate size |
|
|
|
|
|
|
| Allowed materials |
All substrates Film or pattern of all types |
Silicon, glass, and polymer substrates Film or pattern of all types except type IV |
Hotplate dependent. (All substrates and film or pattern of all types, unless otherwise noted on the hotplate) |
Tool dependent. Typically Silicon, III-V, and glass substrates. |
Silicon, glass, and high Tg polymer substrates Film or pattern of all types |
Silicon, glass, and high Tg polymer substrates Film or pattern of all types except resist |
| Restrictions (Not allowed) |
III-V, copper, steel substrates
Pb, Te films |
Hotplate dependent. Any restrictions will be noted on the hotplate. |
Low Tg polymer, copper, steel substrates. Pb, Te films. |
III-V, low Tg polymer, copper, steel substrates | III-V, low Tg polymer, copper, steel substrates
Resist is not allowed | |
| QC - requires login |
https://labmanager.dtu.dk/view_binary.php?type=data&mach=293 |
Hotplate 1: Hotplate 2:
|
Hotplate: 90-110C: Spin coater: Labspin 02: Spin coater: Labspin 03: |
Spincoater: Gamma ebeam & UV: Spincoater: Gamma UV: Developer: TMAH UV-lithography: Spincoater: Süss stepper: Developer: Stepper:
|
Hotplates
Hotplate: 90-110C

Hotplate: 90-110C is used for baking of 2" - 6" wafers. Do not exceed 120°C.
The user manual, and contact information can be found in LabManager:
Hotplate: 90-110C - requires login
SU-8 hotplates

We have four hotplates dedicated to baking of SU-8.
Hotplate 1 (SU8) and Hotplate 2 (SU8) are located in cleanroom E-4.
Hotplate 3 (SU8) and Hotplate 4 (SU8) are located in PolyFabLab in building 347.
Users can control the ramp-time, the baking temperature, and the baking time.
The hotplates are temperature limited to 180°C.
The user manual, and contact information can be found in LabManager:
Hotplate 1 (SU8) - requires login
Hotplate 2 (SU8) - requires login
Hotplate 3 (SU8) - requires login
Hotplate 4 (SU8) - requires login
Small benchtop hotplates
Model: Präzitherm PZ 28-2.
Contact bake only. Maximum temperature is hotplate dependent.
Most of these hotplates have been fitted with a top-plate in order to protect the original hotplate surface. With the top-plate, the set point of the controller must be adjusted in order to achieve the correct temperature during the bake:
Actual surface temperature = 0.9 * display value
Gamma hotplates

Hotplate temperatures are recipe dependent.
Information about the Süss MicroTec Gamma tools can be found in labadviser:
- Spin Coater: Gamma UV
- Spin Coater: Gamma e-beam & UV
- Developer TMAH UV-lithography
- Spin Coater: Süss Stepper
- Developer: TMAH Stepper
Ovens
Oven: 110C - 250C

Variable temperature convection oven mostly used for baking of wafers as a hard baking step after development of photoresist.
The set-point can be varied, but should always be returned to 110°C after use.
The user manual, and contact information can be found in LabManager:
Oven: 110C - 250C - requires login
Oven 250C

The oven is typically used for dehydration pretreatment, of Si and glass substrates, to promote the resist adhesion. We recommend placing the wafers in a metal carrier in the oven for at least for 4 hours, or overnight, and spin coat resist on them as soon as possible after removing them from the oven.
The user manual, and contact information can be found in LabManager:
Oven 250C - requires login