Jump to content

Specific Process Knowledge/Lithography/UVExposure: Difference between revisions

Jehem (talk | contribs)
Jehem (talk | contribs)
No edit summary
 
(161 intermediate revisions by 3 users not shown)
Line 1: Line 1:
'''Feedback to this page''': '''[mailto:photolith@nanolab.dtu.dk?Subject=Feed%20back%20from%20page%20http://labadviser.nanolab.dtu.dk/index.php/Specific_Process_Knowledge/Lithography/UVExposure click here]'''
{{cc-nanolab}}


[[Category: Equipment |Lithography exposure]]
[[Category: Equipment|Lithography exposure]]
[[Category: Lithography|Exposure]]
[[Category: Lithography|Exposure]]


== UV Exposure Comparison Table ==
__TOC__
 
 
{| border="2" cellspacing="0" cellpadding="2"
 
!colspan="2" border="none" style="background:silver; color:black;" align="center"|Equipment
|style="background:WhiteSmoke; color:black"|<b>[[Specific_Process_Knowledge/Lithography/UVExposure#KS Aligner|KS Aligner]]</b>
|style="background:WhiteSmoke; color:black"|<b>[[Specific_Process_Knowledge/Lithography/UVExposure#Aligner:_MA6_-_2|Aligner: MA6 - 2]]</b>
|style="background:WhiteSmoke; color:black"|<b>[[Specific_Process_Knowledge/Lithography/UVExposure#Aligner: Maskless 01|Aligner: Maskless 01]]</b>
|style="background:WhiteSmoke; color:black"|<b>[[Specific_Process_Knowledge/Lithography/UVExposure#Aligner: Maskless 02|Aligner: Maskless 02]]</b>
|style="background:WhiteSmoke; color:black"|<b>[[Specific_Process_Knowledge/Lithography/UVExposure#Aligner: Maskless 03|Aligner: Maskless 03]]</b>
|style="background:WhiteSmoke; color:black"|<b>[[Specific_Process_Knowledge/Lithography/UVExposure#Inclined UV Lamp|Inclined UV Lamp]]</b>


=UV Exposure Comparison Table=
{| class="wikitable"
|-
!
! [[Specific_Process_Knowledge/Lithography/UVExposure/aligner_MA6-1|Aligner: MA6-1]]
! [[Specific_Process_Knowledge/Lithography/UVExposure/aligner_MA6-2|Aligner: MA6-2]]
! [[Specific_Process_Knowledge/Lithography/UVExposure/aligner_MLA1|Aligner: Maskless 01]]
! [[Specific_Process_Knowledge/Lithography/UVExposure/aligner_MLA2|Aligner: Maskless 02]]
! [[Specific_Process_Knowledge/Lithography/UVExposure/aligner_MLA3|Aligner: Maskless 03]]
! [[Specific_Process_Knowledge/Lithography/UVExposure/aligner_MLA4|Aligner: Maskless 04]]
|-
|-
!style="background:silver; width:100px; color:black;" align="center"|Purpose  
! scope=row| Purpose
|style="background:LightGrey; color:black"|
|
|style="background:WhiteSmoke; color:black"|
*Top side alignment
*Top Side Alignment
*Back side alignment
*Back Side Alignment
*UV exposure
*UV exposure
|style="background:WhiteSmoke; color:black"|
NB: this tool is in PolyFabLab
*Top Side Alignment
|
*Back Side Alignment
*Top side alignment
*Back side alignment
*UV exposure
*UV exposure
*(DUV exposure)
*Bond alignment
*Bond alignment
|style="background:WhiteSmoke; color:black"|
|
*Top Side Alignment
*Top side alignment
*Maskless UV exposure
|
*Top side alignment
*Back side alignment
*Maskless UV exposure
*Maskless UV exposure
|style="background:WhiteSmoke; color:black"|
|
*Top Side Alignment
*Top side alignment
*Back Side Alignment
*Back side alignment
*Maskless UV exposure
*Maskless UV exposure
|style="background:WhiteSmoke; color:black"|
|
*Top Side Alignment
*Top side alignment
*Back Side Alignment
*Maskless UV exposure
*Maskless UV exposure
|style="background:WhiteSmoke; color:black"|
*Direct laser writing
*UV exposure
NB: this tool is in PolyFabLab
*DUV exposure
|-
 
! scope=row| Minimum feature size
| ~1 µm || ~1 µm || ~1 µm || ~1 µm || ~1 µm || ~1 µm
|-
|-
!style="background:silver; color:black" align="center" valign="center" rowspan="3"|Performance
! scope=row| Alignment accuracy
|style="background:LightGrey; color:black"|Minimum feature size
|
|style="background:WhiteSmoke; color:black"|
*TSA: ±2 µm
*1.5µm down to 1µm
*BSA: ±5 µm
|style="background:WhiteSmoke; color:black"|
|
*1.5µm down to 0.5µm
*TSA: ±1 µm
|style="background:WhiteSmoke; color:black"|
*BSA: ±2 µm
*2µm down to 1µm
|
|style="background:WhiteSmoke; color:black"|
±2 µm<br>(±1 µm possible)
*1µm down to 0.6µm
|
|style="background:WhiteSmoke; color:black"|
*TSA: ± 0.5 µm
*2µm down to 1µm
*BSA: ± 1 µm
|style="background:WhiteSmoke; color:black"|
|
*TSA: ± 0.5 µm
*BSA: ± 1 µm
|
±1 µm
|-
|-
|style="background:LightGrey; color:black"|Exposure light/filters/spectrum
! scope=row| Exposure light source
|style="background:WhiteSmoke; color:black"|
|
*350W Hg lamp
*350 W Hg lamp
*i-line filter (365nm notch filter), intensity in Constant Intensity mode: 8mW/cm<sup>2</sup> @ 365nm
*i-line filter (365nm band pass filter)
*303nm filter optional
|
|style="background:WhiteSmoke; color:black"|
*500 W Hg-Xe lamp
*500W Hg-Xe lamp
*i-line filter (365nm band pass filter)
*i-line filter (365nm notch filter), intensity in Constant Intensity mode: 11mW/cm<sup>2</sup> @ 365nm
|
*UV350 optics optional
365 nm LED
*UV250 optics optional
|
|style="background:WhiteSmoke; color:black"|
375 nm laser diode array
*365nm LED
|
|style="background:WhiteSmoke; color:black"|
405 nm laser diode array
*375nm laserdiodes
|
or
*365 nm LED
*405nm laserdiodes
*405 nm laser diode
|style="background:WhiteSmoke; color:black"|
*405nm laserdiodes
|style="background:WhiteSmoke; color:black"|
*1000 W Hg-Xe lamp
*near UV (350-450nm), mid UV (260-320nm), and deep UV (220-260nm)
 
|-
|-
|style="background:LightGrey; color:black"|Exposure mode
! scope=row| Exposure mode
|style="background:WhiteSmoke; color:black"|
|
*Flood exposure
*Proximity
*Proximity
*Contact
*Contact:
**Soft contact
**Soft contact
**Hard contact
**Hard contact
**Vacuum contact
**Vacuum contact
|style="background:WhiteSmoke; color:black"|
|
*Flood exposure
*Proximity
*Proximity
*Contact
*Contact:
**Soft contact
**Soft contact
**Hard contact
**Hard contact
**Vacuum contact
**Vacuum contact
|style="background:WhiteSmoke; color:black"|
|
*Projection  
*Projection:
**Pneumatic auto-focus
|
*Projection:
**Optical auto-focus
**Pneumatic auto-focus
|
*Projection:
**Pneumatic auto-focus
**Pneumatic auto-focus
|style="background:WhiteSmoke; color:black"|
|
*Projection  
*Projection:
**Optical auto-focus
**Optical auto-focus
**Pneumatic auto-focus
**Pneumatic auto-focus
|style="background:WhiteSmoke; color:black"|
*Direct laser writing:
*Projection
**Optical auto-focus
**Pneumatic auto-focus
**Pneumatic auto-focus
|style="background:WhiteSmoke; color:black"|
*Flood exposure
*Proximity exposure with home-made chuck and maskholder
*Inclined exposure
*Rotating exposure
|-
|-
!style="background:silver; color:black" align="center" valign="center" rowspan="3"|Substrates
! scope=row| Batch size
|style="background:LightGrey; color:black"|Batch size
| 1 || 1 || 1 || 1 || 1 || 1
|style="background:WhiteSmoke; color:black"|
*1 small sample, down to 10x10 mm<sup>2</sup>
*1 50 mm wafer
*1 100 mm wafer
*1 150 mm wafer
|style="background:WhiteSmoke; color:black"|
*1 small sample, down to 10x10 mm<sup>2</sup>
*1 50 mm wafer
*1 100 mm wafer
*1 150 mm wafer
|style="background:WhiteSmoke; color:black"|
*1 small sample, down to 5x5 mm<sup>2</sup>
*1 50 mm wafer
*1 100 mm wafer
*1 150 mm wafer
|style="background:WhiteSmoke; color:black"|
*1 small sample, down to 3x3 mm<sup>2</sup>
*1 50 mm wafer
*1 100 mm wafer
*1 150 mm wafer
*1 200 mm wafer
|style="background:WhiteSmoke; color:black"|
*1 small sample, down to 5x5 mm<sup>2</sup>
*1 50 mm wafer
*1 100 mm wafer
*1 150 mm wafer
|style="background:WhiteSmoke; color:black"|
*all sizes up to 8inch
|-
|-
| style="background:LightGrey; color:black"|Allowed materials
! scope=row| Allowed materials
|style="background:WhiteSmoke; color:black"|
| All PolyFabLab materials
*All cleanroom materials except copper and steel
|
*Dedicated 2inch chuck for III-V materials
|style="background:WhiteSmoke; color:black"|
*All cleanroom materials except copper and steel
*All cleanroom materials except copper and steel
*Dedicated chuck for III-V materials
*Dedicated chuck for III-V materials
|style="background:WhiteSmoke; color:black"|
| All cleanroom materials
*All cleanroom materials
| All cleanroom materials
|style="background:WhiteSmoke; color:black"|
| All cleanroom materials
*All cleanroom materials
| All PolyFabLab materials
|style="background:WhiteSmoke; color:black"|
*All cleanroom materials
|style="background:WhiteSmoke; color:black"|
*All cleanroom materials
|-
|}
 
 
==KS Aligner==
[[Image:KSAligner in E-4.jpg|300x300px|thumb|The KS Aligner is placed in E-4]]
 
'''Feedback to this section''': '''[mailto:labadviser@nanolab.dtu.dk?Subject=Feed%20back%20from%20page%20http://labadviser.nanolab.dtu.dk/index.php/Specific_Process_Knowledge/Lithography/UVExposure#KS_Aligner click here]'''
 
SUSS Mask Aligner MA6 is designed for high resolution photolithography.
The 365nm exposure wavelength version is capable of 1.25 (1.0) um resolution in vacuum contact. All contact exposure programs (vacuum, hard, soft, proximity) are supplied.
Two alignment options are available: top side alignment (TSA) with a split field or a video microscope and back side alignment (BSA) with BSA microscope. It is also possible to make IR- light alignment.
 
'''Training videos: [https://www.youtube.com/watch?v=o8IBtfQHNzU Operation] [https://www.youtube.com/watch?v=rvUuXYgw-xU Alignment]''' (on Aligner: MA6-2, but KS Aligner is the same model)
 
'''The user manual(s), quality control procedure(s) and results and contact information can be found in [http://labmanager.dtu.dk/function.php?module=Machine&view=view&mach=44 LabManager].'''
 
===Process information===
The KS Aligner has an i-line notch filter installed. This results in an exposure light peak around 365nm with a FWHM of 7nm.
 
*[[Specific Process Knowledge/Lithography/Resist#KS_Aligner|Information on UV exposure dose]]
 
===Quality Control (QC)===
{| border="1" cellspacing="2" cellpadding="2" colspan="3"
|bgcolor="#98FB98" |'''Quality Control (QC) for KS Aligner'''
|-
|
*[http://labmanager.dtu.dk/d4Show.php?id=5644&mach=44 The QC procedure for KS Aligner]<br>
*[https://labmanager.dtu.dk/view_binary.php?type=data&mach=44 The newest QC data for KS Aligner]
{| {{table}}
| align="center" |
{| border="1" cellspacing="1" cellpadding="2"  align="center" style="width:300px"
 
! QC Recipe:
! Manual intensity measurement
|-
|Measurement area
|4"
|-
|Number of measurements
|5
|-
|}
| align="center" valign="top"|
{| border="2" cellspacing="1" cellpadding="2" align="center" style="width:400px"
!QC limits
!KS Aligner
|-
|Nominal intensity
|8 mW/cm<sup>2</sup> @ 365 nm
|-
|Intensity deviation from nominal
|≤5%
|-
|Intensity non-uniformity
|≤2%
|-
|}
|-
|}
Power supply and/or lamp will be adjusted if intensity is outside the limit.
|}
 
===Equipment performance and process related parameters===
 
{| border="2" cellspacing="0" cellpadding="2"
 
 
!style="background:silver; color:black;" align="center" width="60"|Purpose
|style="background:LightGrey; color:black"|
|style="background:WhiteSmoke; color:black" align="center" colspan="2"|
Alignment and UV exposure
|-
 
!style="background:silver; color:black" align="left" valign="center" rowspan="5"|Performance
 
|style="background:LightGrey; color:black"|Exposure mode
|style="background:WhiteSmoke; color:black" align="center" colspan="2"|
vacuum contact, hard contact, soft contact, proximity, flood exposure
|-
| style="background:LightGrey; color:black"|Exposure light/filters
|style="background:WhiteSmoke; color:black" align="center" colspan="2"|
*broadband (i-, g-, h-line)
*365 nm (i-line)
*303 nm
|-
|style="background:LightGrey; color:black"|Minimum structure size
|style="background:WhiteSmoke; color:black" align="center" colspan="2"|
down to 1.25µm
|-
|style="background:LightGrey; color:black"|Mask size
|style="background:WhiteSmoke; color:black" align="center" colspan="2"|
*5x5 inch
*7x7 inch
*special holder for 4 x 2" designs on 5x5 inch
|-
|style="background:LightGrey; color:black"|Alignment modes
|style="background:WhiteSmoke; color:black" align="center" colspan="2"|
*Top side (TSA)
*Backside (BSA)
|-
!style="background:silver; color:black" align="center" valign="center" rowspan="3"|Substrates
|style="background:LightGrey; color:black"|Substrate size
|style="background:WhiteSmoke; color:black" align="center" colspan="2"|
* small pieces 1x1cm
* 50 mm wafers
* 100 mm wafers
* 150 mm wafers
|-
| style="background:LightGrey; color:black"|Allowed materials
|style="background:WhiteSmoke; color:black" align="center" colspan="2"|
All cleanroom materials
 
Dedicated chuck for III-V materials
|-
|style="background:LightGrey; color:black"|Batch
|style="background:WhiteSmoke; color:black" align="center" colspan="2"|
1
|-
|}
 
<br clear="all" />
 
==Aligner: MA6 - 2==
 
[[Image:AlignerMA6-2 in E-4.jpg|300x300px|thumb|The Aligner: MA6 - 2 is placed in E-4]]
 
'''Feedback to this section''': '''[mailto:labadviser@nanolab.dtu.dk?Subject=Feed%20back%20from%20page%20http://labadviser.nanolab.dtu.dk/index.php/Specific_Process_Knowledge/Lithography/UVExposure#Aligner:_MA6_-_2 click here]'''
 
The Süss MicroTek Mask Aligner MA6 is designed for high resolution photolithography.
The 365nm exposure wavelength version is capable of 1.25 (1.0) um resolution in vacuum contact. All contact exposure programs (vacuum, low vacuum, hard, soft, proximity) are supplied.
Two alignment options are available: top side alignment (TSA) with a split field or a video microscope and back side alignment (BSA) with BSA (video) microscope.
 
The aligner can also be used for bond alignment (for Wafer Bonder 02). Special training is required.
 
'''Training videos: [https://www.youtube.com/watch?v=o8IBtfQHNzU Operation] [https://www.youtube.com/watch?v=rvUuXYgw-xU Alignment]'''
 
'''The user manual, quality control procedures and results, user APVs, and contact information can be found in [http://labmanager.dtu.dk/function.php?module=Machine&view=view&mach=339 LabManager].'''
 
===Process information===
The Aligner: MA6 - 2 has an i-line notch filter installed. This results in an exposure light peak at 365nm. Compared to exposure on the KS Aligner, the optimal dose should be very similar. The 500W Hg-Xe lamp also enables exposure in the DUV range around 240nm. This functionality is not established yet, partly due to safety concerns.
 
*[[Specific Process Knowledge/Lithography/Resist#Aligner:_MA6_-_2|Information on UV exposure dose]]
 
===Quality Control (QC)===
{| border="1" cellspacing="2" cellpadding="2" colspan="3"
|bgcolor="#98FB98" |'''Quality Control (QC) for Aligner: MA6-2'''
|-
|
*[http://labmanager.dtu.dk/d4Show.php?id=5644&mach=339 The QC procedure for Aligner: MA6-2]<br>
*[https://labmanager.dtu.dk/view_binary.php?type=data&mach=339 The newest QC data for Aligner: MA6-2]
{| {{table}}
| align="center" |
{| border="1" cellspacing="1" cellpadding="2"  align="center" style="width:300px"
 
! QC Recipe:
! Manual intensity measurement
|-
|Measurement area
|4"
|-
|Number of measurements
|5
|-
|}
| align="center" valign="top"|
{| border="2" cellspacing="1" cellpadding="2" align="center" style="width:400px"
!QC limits
!Aligner: MA6-2
|-
|Nominal intensity
|11 mW/cm<sup>2</sup> @ 365 nm
|-
|Intensity deviation from nominal
|≤5%
|-
|Intensity non-uniformity
|≤2%
|-
|}
|-
|}
Power supply and/or lamp will be adjusted if intensity is outside the limit.
|}
 
===Alignment===
 
'''Top Side Alignment:'''
*TSA microscope standard objectives: 5X, and 10X (20X available)
*TSA microscope special objectives: 11.25X offset (for smaller separation)
 
*Minimum distance between TSA microscope objectives: 33 mm (8 mm for special objectives)
*Maximum distance between TSA microscope objectives: 160 mm
*TSA microscope travel range: X +/- 25mm; Y +20mm / -75mm (towards flat)
 
'''BackSide Alignment:'''
*Minimum distance between BSA microscope objectives: 15 mm
*Maximum distance between BSA microscope objectives: 100 mm
*BSA microscope travel range: X +50mm / -16mm; Y +50mm / -20mm (towards flat)
*BSA chuck view ranges:
**2": X +/-  8-22mm; Y +/- 0-6mm
**4": X +/- 14-46mm; Y +/- 0-10mm
**6": X +/- 14-69mm; Y +/- 0-10mm
 
 
'''Microscope field of view (W x H, splitfield):'''
*TSA 5X
**Oculars: 1.3mm x 2.6mm (Ø2.6mm full field)
**Camera: 350µm x 500µm (700µm x 500µm full field)
*TSA 10X
**Oculars: 0.6mm x 1.3mm (Ø1.3mm full field)
**Camera: 150µm x 250µm (350µm x 250µm full field)
*TSA special
**Oculars: 0.55mm x 1.1mm (Ø1.1mm full field)
**Camera: 150µm x 200µm (300µm x 200µm full field)
*BSA camera
**Low: 1.5mm x 2mm (3mm x 2mm full field)
**High: 450µm x 650µm (950µm x 650µm full field)
 
=== Equipment performance and process related parameters ===
 
{| border="2" cellspacing="0" cellpadding="2"
 
!style="background:silver; color:black;" align="center" width="60"|Purpose
|style="background:LightGrey; color:black"|
|style="background:WhiteSmoke; color:black" align="center" colspan="2"|
Mask alignment and UV exposure, potentially DUV exposure <sup>1)</sup>
 
Bond alignment
|-
 
!style="background:silver; color:black" align="left" valign="center" rowspan="5"|Performance
 
|style="background:LightGrey; color:black"|Exposure mode
|style="background:WhiteSmoke; color:black" align="center" colspan="2"|
vacuum contact, hard contact, soft contact, proximity, flood exposure
|-
| style="background:LightGrey; color:black"|Exposure light/filters
|style="background:WhiteSmoke; color:black" align="center" colspan="2"|
*broadband (i-, g-, h-line)
*365 nm (i-line)
*"UV300" (280-350 nm)
*DUV (240 nm) <sup>1)</sup>
|-
|style="background:LightGrey; color:black"|Minimum structure size
|style="background:WhiteSmoke; color:black" align="center" colspan="2"|
Typically 1.25 µm, possibly down to 0.8 µm <sup>1)</sup>
|-
|style="background:LightGrey; color:black"|Mask size
|style="background:WhiteSmoke; color:black" align="center" colspan="2"|
*5x5 inch
*7x7 inch
*special holder for 4 x 2" designs on 5x5 inch
|-
|style="background:LightGrey; color:black"|Alignment modes
|style="background:WhiteSmoke; color:black" align="center" colspan="2"|
*Top side (TSA)
*Backside (BSA)
|-
!style="background:silver; color:black" align="center" valign="center" rowspan="3"|Substrates
|style="background:LightGrey; color:black"|Substrate size
|style="background:WhiteSmoke; color:black" align="center" colspan="2"|
* small pieces 1x1cm
* 50 mm wafers
* 100 mm wafers
* 150 mm wafers
|-
|-
| style="background:LightGrey; color:black"|Allowed materials
|style="background:WhiteSmoke; color:black" align="center" colspan="2"|
All cleanroom materials except copper and steel
Dedicated chuck for III-V materials
|-
|style="background:LightGrey; color:black"|Batch
|style="background:WhiteSmoke; color:black" align="center" colspan="2"|
1
|-
|}
|}


<sup>1)</sup> Not available yet. Requires tool change. Would require safety investigation (and a dedicated project) to become available.
=Mask vs Maskless aligners=
Comparison study between mask aligners and maskless aligners can be found [[Specific_Process_Knowledge/Lithography/Aligners/MAvsMLA|here]].


<br clear="all" />
=Decommisioned tools=
 
<span style="color:red">Inclined UV lamp was decommissioned 2023.</span>
== Aligner: Maskless 01 ==
 
'''Feedback to this section''': '''[mailto:lithography@Nanolab.dtu.dk?Subject=Feed%20back%20from%20page%20http://labadviser.nanolab.dtu.dk/index.php/Specific_Process_Knowledge/Lithography/UVExposure#Aligner:_Maskless_01 click here]'''
 
[[Image:Heidelberg_MLA100.jpg|300x300px|thumb|Aligner: Maskless 01 positioned in E-5 (2017)]]
 
The logon password for the PC is "mla" (without quotation marks).
 
The MLA 100 Maskless Aligner located in the E-4 cleanroom is a direct exposure lithography tool installed in 2017.
It is a UV LED exposure system, that exposes the patterns directly on photosensitive resists on chips, 2, 4, and 6 inch substrates, without prior fabrication of the mask.
The system offers top side alignment with high accuracy.
 
'''The user manual and contact information can be found in LabManager:'''
Equipment info in [http://labmanager.dtu.dk/function.php?module=Machine&view=view&mach=422 LabManager]
 
*[[Specific Process Knowledge/Lithography/Resist#Aligner:_Maskless_01|Information on UV exposure dose]]
 
===[[Specific Process Knowledge/Lithography/Aligners/Aligner: Maskless 01 processing|Process information]]===
 
[[Specific_Process_Knowledge/Lithography/Aligners/Aligner:_Maskless_01_processing#Exposure_technology|Exposure technology]]
 
[[Specific_Process_Knowledge/Lithography/Aligners/Aligner:_Maskless_01_processing#Process_Parameters|Process parameters]]
 
[[Specific_Process_Knowledge/Lithography/Aligners/Aligner:_Maskless_01_processing#Substrate_positioning|Substrate positioning]]
 
[[Specific_Process_Knowledge/Lithography/Aligners/Aligner:_Maskless_01_processing#Alignment|Alignment]]
 
[[Specific_Process_Knowledge/Lithography/Aligners/Aligner:_Maskless_01_processing#Optimal_use_of_the_maskless_aligner|Optimal use of the maskless aligner]]
 
=== Equipment performance and process related parameters ===
 
{| border="2" cellspacing="0" cellpadding="2"
 
 
!style="background:silver; color:black;" align="center" width="60"|Purpose
|style="background:LightGrey; color:black"|
|style="background:WhiteSmoke; color:black" align="center" colspan="2"|
Alignment and UV exposure
|-
 
!style="background:silver; color:black" align="left" valign="center" rowspan="6"|Performance
 
|style="background:LightGrey; color:black"|Exposure mode
|style="background:WhiteSmoke; color:black" align="center" colspan="2"|
Projection
|-
| style="background:LightGrey; color:black"|Exposure light
|style="background:WhiteSmoke; color:black" align="center" colspan="2"|
365nm (LED), FWHM=8nm
|-
|style="background:LightGrey; color:black"|Focusing method
|style="background:WhiteSmoke; color:black" align="center" colspan="2"|
Pneumatic
|-
|style="background:LightGrey; color:black"|Minimum structure size
|style="background:WhiteSmoke; color:black" align="center" colspan="2"|
down to 1µm
|-
|style="background:LightGrey; color:black"|Design formats
|style="background:WhiteSmoke; color:black" align="center" colspan="2"|
*'''GDS-II'''
*CIF
*DXF
*Gerber
*HIMT format
|-
|style="background:LightGrey; color:black"|Alignment modes
|style="background:WhiteSmoke; color:black" align="center" colspan="2"|
Top side only
 
|-
!style="background:silver; color:black" align="center" valign="center" rowspan="3"|Substrates
|style="background:LightGrey; color:black"|Substrate size
|style="background:WhiteSmoke; color:black" align="center" colspan="2"|
* maximum writing area: 125x125 mm<sup>2</sup>
* 150 mm wafer
* 100 mm wafer
* 50 mm wafer
* pieces down to 5x5 mm<sup>2</sup>
|-
| style="background:LightGrey; color:black"|Allowed materials
|style="background:WhiteSmoke; color:black" align="center" colspan="2"|
All cleanroom materials
|-
|style="background:LightGrey; color:black"|Batch
|style="background:WhiteSmoke; color:black" align="center" colspan="2"|
1
|-
|}
 
<br clear="all" />
 
==Aligner: Maskless 02==
'''Feedback to this section''': '''[mailto:lithography@Nanolab.dtu.dk?Subject=Feed%20back%20from%20page%20http://labadviser.nanolab.dtu.dk/index.php/Specific_Process_Knowledge/Lithography/UVExposure#Aligner:_Maskless_02 click here]'''
 
MLA150 WMI maskless aligner from Heidelberg Instruments GmbH.
 
'''PC logon password'''
The logon password for the PC is "mla" (without quotation marks).
 
 
'''Special features'''
*High resolution (Write Mode I, Optical Autofocus)
*Backside Alignment
*Basic Gray Scale Exposure
*Advanced Field Alignment Mode for alignment to individual chips/devices on the substrate
*High Aspect Ratio Mode for exposure of thick resists
*Upgrade to 8" (stage and exposure area)
 
 
'''<span style="color:red">Special restrictions</span>'''
*No pneumatic autofocus
*405 nm laser is not allowed
*Soft resists are not allowed
*Resist thickness must be ≤10 µm
*No crystal bonded chips
*Thickness variations across the substrate must be <50 µm
*Wafer bow must be <50 µm
 
 
'''[https://www.youtube.com/playlist?list=PLjWVU97LayHAiCabstMfAUeeWyQoQI_cV Training videos]'''
 
Equipment info in [http://labmanager.dtu.dk/function.php?module=Machine&view=view&mach=440 LabManager]
 
===[[Specific Process Knowledge/Lithography/Aligners/Aligner: Maskless 02 processing|Process information]]===
 
[[Specific_Process_Knowledge/Lithography/Aligners/Aligner:_Maskless_02_processing#Exposure_technology|Exposure technology]]
 
[[Specific_Process_Knowledge/Lithography/Aligners/Aligner:_Maskless_02_processing#Process_Parameters|Process Parameters]]
 
[[Specific_Process_Knowledge/Lithography/Aligners/Aligner:_Maskless_02_processing#Features|Features]]
 
[[Specific_Process_Knowledge/Lithography/Aligners/Aligner:_Maskless_02_processing#Alignment|Alignment]]
 
=== Equipment performance and process related parameters ===
 
{| border="2" cellspacing="0" cellpadding="2"
 
 
!style="background:silver; color:black;" align="center" width="60"|Purpose
|style="background:LightGrey; color:black"|
|style="background:WhiteSmoke; color:black" align="center" colspan="2"|
Alignment and UV exposure
|-
 
!style="background:silver; color:black" align="left" valign="center" rowspan="6"|Performance
 
|style="background:LightGrey; color:black"|Exposure mode
|style="background:WhiteSmoke; color:black" align="center" colspan="2"|
Projection
|-
| style="background:LightGrey; color:black"|Exposure light
|style="background:WhiteSmoke; color:black" align="center" colspan="2"|
*375 nm
*<s>405 nm</s> NOT ALLOWED
(laser diode arrays)
|-
|style="background:LightGrey; color:black"|Focusing method
|style="background:WhiteSmoke; color:black" align="center" colspan="2"|
*Optical
*<s>Pneumatic</s> DISABLED
|-
|style="background:LightGrey; color:black"|Minimum structure size
|style="background:WhiteSmoke; color:black" align="center" colspan="2"|
down to 600nm <sup>1)</sup>
|-
|style="background:LightGrey; color:black"|Design formats
|style="background:WhiteSmoke; color:black" align="center" colspan="2"|
*'''GDS-II'''
*CIF
*DXF
*Gerber
*HIMT format
|-
|style="background:LightGrey; color:black"|Alignment modes
|style="background:WhiteSmoke; color:black" align="center" colspan="2"|
*Top side alignment
*Backside alignment
*Field alignment (chip-by-chip TSA)
 
|-
!style="background:silver; color:black" align="center" valign="center" rowspan="3"|Substrates
|style="background:LightGrey; color:black"|Substrate size
|style="background:WhiteSmoke; color:black" align="center" colspan="2"|
* maximum writing area: 200x200 mm<sup>2</sup>
* 200 mm wafer
* 150 mm wafer
* 100 mm wafer
* 50 mm wafer
* pieces down to 3x3 mm<sup>2</sup> <sup>1)</sup>
|-
| style="background:LightGrey; color:black"|Allowed materials
|style="background:WhiteSmoke; color:black" align="center" colspan="2"|
All cleanroom materials
|-
|style="background:LightGrey; color:black"|Batch
|style="background:WhiteSmoke; color:black" align="center" colspan="2"|
1
|-
|}
 
<sup>1)</sup> with optical autofocus
 
<br clear="all" />
 
==Aligner: Maskless 03==
 
'''Feedback to this section''': '''[mailto:lithography@nanolab.dtu.dk?Subject=Feed%20back%20from%20page%20http://labadviser.nanolab.dtu.dk/index.php/Specific_Process_Knowledge/Lithography/UVExposure#Aligner:_Maskless_03 click here]'''
 
MLA150 WMII maskless aligner from Heidelberg Instruments GmbH.
 
The logon password for the PC is "mla" (without quotation marks).
 
Special features:
*Backside Alignment
*Advanced Field Alignment Mode for alignment to individual chips/devices on the substrate
*Separate conversion PC (Power PC)
 
 
'''[https://www.youtube.com/playlist?list=PLjWVU97LayHAiCabstMfAUeeWyQoQI_cV Training videos]'''
 
Equipment info in [http://labmanager.dtu.dk/function.php?module=Machine&view=view&mach=464 LabManager]
 
===[[Specific Process Knowledge/Lithography/Aligners/Aligner: Maskless 03 processing|Process information]]===
 
[[Specific_Process_Knowledge/Lithography/Aligners/Aligner:_Maskless_03_processing#Exposure_technology|Exposure technology]]
 
[[Specific_Process_Knowledge/Lithography/Aligners/Aligner:_Maskless_03_processing#Process_Parameters|Process Parameters]]
 
[[Specific_Process_Knowledge/Lithography/Aligners/Aligner:_Maskless_03_processing#Features|Features]]
 
[[Specific_Process_Knowledge/Lithography/Aligners/Aligner:_Maskless_03_processing#Alignment|Alignment]]
 
=== Equipment performance and process related parameters ===
 
{| border="2" cellspacing="0" cellpadding="2"
 
 
!style="background:silver; color:black;" align="center" width="60"|Purpose
|style="background:LightGrey; color:black"|
|style="background:WhiteSmoke; color:black" align="center" colspan="2"|
Alignment and UV exposure
|-
 
!style="background:silver; color:black" align="left" valign="center" rowspan="6"|Performance
 
|style="background:LightGrey; color:black"|Exposure mode
|style="background:WhiteSmoke; color:black" align="center" colspan="2"|
Projection
|-
| style="background:LightGrey; color:black"|Exposure light
|style="background:WhiteSmoke; color:black" align="center" colspan="2"|
405nm (laser diode array)
|-
|style="background:LightGrey; color:black"|Focusing method
|style="background:WhiteSmoke; color:black" align="center" colspan="2"|
Pneumatic
|-
|style="background:LightGrey; color:black"|Minimum structure size
|style="background:WhiteSmoke; color:black" align="center" colspan="2"|
down to 1µm
|-
|style="background:LightGrey; color:black"|Design formats
|style="background:WhiteSmoke; color:black" align="center" colspan="2"|
*'''GDS-II'''
*CIF
*DXF
*Gerber
*HIMT format
|-
|style="background:LightGrey; color:black"|Alignment modes
|style="background:WhiteSmoke; color:black" align="center" colspan="2"|
*Top side alignment
*Backside alignment
*Field alignment (chip-by-chip TSA)
 
|-
!style="background:silver; color:black" align="center" valign="center" rowspan="3"|Substrates
|style="background:LightGrey; color:black"|Substrate size
|style="background:WhiteSmoke; color:black" align="center" colspan="2"|
* maximum writing area: 150x150 mm<sup>2</sup>
* 150 mm wafer
* 100 mm wafer
* 50 mm wafer
* pieces down to 5x5 mm<sup>2</sup>
|-
| style="background:LightGrey; color:black"|Allowed materials
|style="background:WhiteSmoke; color:black" align="center" colspan="2"|
All cleanroom materials
|-
|style="background:LightGrey; color:black"|Batch
|style="background:WhiteSmoke; color:black" align="center" colspan="2"|
1
|-
|}
 
<br clear="all" />
 
==Inclined UV Lamp==
 
'''Feedback to this section''': '''[mailto:labadviser@nanolab.dtu.dk?Subject=Feed%20back%20from%20page%20http://labadviser.nanolab.dtu.dk/index.php/Specific_Process_Knowledge/Lithography/UVExposure#Inclined_UV_lamp click here]'''
 
[[Image:Inclined UV lamp_1.jpg|300x300px|right|thumb|Inclined UV lamp is placed in CX-1]]
 
The Inclined UV lamp is 1000 W Hg(Xe)lamp source designed for near UV, 350-450nm, mid UV, 260-320nm, and deep UV, 220-260nm exposures of resists and polymers. The exposure source can be also used to make an inclined exposure in air or in the media tank.
 
The tool was purchased in February 2009 from Newport. The exposure lamp has a official name: Oriel Flood Exposure Source, unit 92540. All other parts of equipment: substrate and mask holder with media tank, exhaust box around the tool, timer controller, were designed and build at DTU Nanolab workshop.
 
The substrate and mask holder with a media tank was designed as part of Master Thesis of DTU Nanotech, Andres Kristensen group. The exhaust box was made as part of safety and the timer controller was build to control exposure time.
 
The technical specification and the general outline of the equipment can be found in LabManager. 
 
'''The user manual(s), quality control procedure(s) and results and contact information can be found in [http://labmanager.dtu.dk/function.php?module=Machine&view=view&mach=259 LabManager].'''
 
<br clear="all" />
 
=== Equipment performance and process related parameters ===
 
{| border="2" cellspacing="0" cellpadding="2"
 
 
!style="background:silver; color:black;" align="center" width="60"|Purpose
|style="background:LightGrey; color:black"|
|style="background:WhiteSmoke; color:black" align="center" colspan="2"|
UV exposure
|-
 
!style="background:silver; color:black" align="left" rowspan="5"|Performance
 
|style="background:LightGrey; color:black"|Exposure mode
|style="background:WhiteSmoke; color:black" align="center" colspan="2"|
*Flood exposure
*Proximity exposure with mask possible for 4inch substrate
*Inclined exposure
*Rotating exposure
|-
| style="background:LightGrey; color:black"|Exposure light/filters
|style="background:WhiteSmoke; color:black" align="center" colspan="2"|
* Near UV(350-450nm)
* Mid UV (260-320nm)
* Deep UV(220-260nm)
 
|-
|style="background:LightGrey; color:black"|Minimum structure size
|style="background:WhiteSmoke; color:black" align="center" colspan="2"|
 
|-
|style="background:LightGrey; color:black"|Mask size
|style="background:WhiteSmoke; color:black" align="center" colspan="2"|
5x5inch optinal
|-
|style="background:LightGrey; color:black"|Alignment modes
|style="background:WhiteSmoke; color:black" align="center" colspan="2"|
No alignment possible
 
|-
!style="background:silver; color:black" align="center" valign="center" rowspan="3"|Substrates
|style="background:LightGrey; color:black"|Substrate size
|style="background:WhiteSmoke; color:black" align="center" colspan="2"|
Up to 8inch substrates, different shapes
|-
| style="background:LightGrey; color:black"|Allowed materials
|style="background:WhiteSmoke; color:black" align="center" colspan="2"|
All cleanroom materials
|-
|style="background:LightGrey; color:black"|Batch
|style="background:WhiteSmoke; color:black" align="center" colspan="2"|
1
|-
|}


<br clear="all" />
[[Specific Process Knowledge/Lithography/UVExposure/aligner_inclinedUV|Information about decommissioned tool can be found here.]]