==Development Comparison Table==
=Development Comparison Table=
 
{| class="wikitable"
{|border="1" cellspacing="1" cellpadding="10" style="text-align:left;"
|-
 
!
!colspan="2" border="none" style="background:silver; color:black;" align="center"|Equipment
! [[Specific Process Knowledge/Lithography/Development/beaker_developer|Manual beaker development]]
|style="background:WhiteSmoke; color:black"|<b>[[Specific_Process_Knowledge/Lithography/Development#Developer: SU8 (Wet Bench)|Developer: SU8 (Wet bench)]]</b>
! [[Specific_Process_Knowledge/Lithography/Development/SU8_developer|Developer: SU8 (Wet bench)]]
|style="background:WhiteSmoke; color:black"|<b>[[Specific_Process_Knowledge/Lithography/Development#Developer: E-beam 02|Developer: E-beam 02]]</b>
! [[Specific_Process_Knowledge/Lithography/Development/manualEbeam_developer|Developer: E-beam 02]]
|style="background:WhiteSmoke; color:black"|<b>[[Specific_Process_Knowledge/Lithography/Development#Developer:_TMAH_Manual 02|Developer: TMAH Manual 02]]</b>
! [[Specific_Process_Knowledge/Lithography/Development/manualTMAH_developer|Developer: TMAH Manual 02]]
|style="background:WhiteSmoke; color:black"|<b>[[Specific_Process_Knowledge/Lithography/Development#Developer_TMAH_UV-lithography|Developer: TMAH UV-lithography]]</b>
! [[Specific_Process_Knowledge/Lithography/Development/UV_developer|Developer: TMAH UV-lithography]]
|style="background:WhiteSmoke; color:black"|<b>[[Specific_Process_Knowledge/Lithography/Development/DUV_developer#Developer:_TMAH_Stepper|Developer: TMAH Stepper]]</b>
! [[Specific_Process_Knowledge/Lithography/Development/DUV_developer|Developer: TMAH Stepper]]
 
|-
|-
!style="background:silver; color:black" align="center" width="60"|Purpose  
! scope=row style="text-align: left;" | Purpose  
|style="background:LightGrey; color:black"|
|
Fall-back option if you have a process, which is not compatible with the automatic, or semi-automatic, tools


 
<span style="color:red">Requires individual risk assessment for TMAH development!</span>
|style="background:WhiteSmoke; color:black"|
|
Development of:
Development of:
*SU-8
*SU-8
|style="background:WhiteSmoke; color:black"|
|
Development of:
Development of:
*ZEP 520A
*ZEP 520A
*AR-P 6200.xx (CSAR)
*AR-P 6200.xx (CSAR)
|style="background:WhiteSmoke; color:black"|
|  
Development of:
Development of:
*AZ nLOF
*AZ nLOF
Line 38: Line 38:
*AZ 4562
*AZ 4562
*DUV resists
*DUV resists
|style="background:WhiteSmoke; color:black"|
|  
Development of:
Development of:
*AZ nLOF
*AZ nLOF
Line 46: Line 46:
*DUV resists
*DUV resists
Post-exposure baking
Post-exposure baking
|style="background:WhiteSmoke; color:black"|
|
Development of:
Development of:
*DUV resists
*DUV resists
Post-exposure baking
Post-exposure baking
|-
|-
!style="background:silver; color:black" align="center" width="60"|Developer  
! scope=row style="text-align: left;" | Developer
|style="background:LightGrey; color:black"|
| Process dependent
 
| mr-Dev 600 (PGMEA)
|style="background:WhiteSmoke; color:black"|
|  
mr-Dev 600 (PGMEA)
|style="background:WhiteSmoke; color:black"|
*ZED N-50
*ZED N-50
*AR-600-546
*AR 600-50
|style="background:WhiteSmoke; color:black"|
| AZ 726 MIF (2.38% TMAH in water)
AZ 726 MIF (2.38% TMAH in water)
| AZ 726 MIF (2.38% TMAH in water)
|style="background:WhiteSmoke; color:black"|
| AZ 726 MIF (2.38% TMAH in water)
AZ 726 MIF (2.38% TMAH in water)
|style="background:WhiteSmoke; color:black"|
AZ 726 MIF (2.38% TMAH in water)
 
|-
|-
!style="background:silver; color:black" align="center" valign="center" rowspan="2"|Method
! scope=row style="text-align: left;" | Method
|style="background:LightGrey; color:black"|Development
| Submersion
|style="background:WhiteSmoke; color:black"|
| Submersion
Submersion
| Puddle
|style="background:WhiteSmoke; color:black"|
| Puddle
Spray/Puddle
| Puddle
|style="background:WhiteSmoke; color:black"|
| Puddle
Puddle
|style="background:WhiteSmoke; color:black"|
Puddle
|style="background:WhiteSmoke; color:black"|
Puddle
|-
|-
|style="background:LightGrey; color:black"|Handling
! scope=row style="text-align: left;" | Handling
|style="background:WhiteSmoke; color:black"|
|
Manual handling in beakers
*Chip bucket
*Single wafer carrier
*Single wafer carrier
*Carrier for up to 5 wafers
|
*Chip bucket
*Chip bucket
*100 mm carrier for up to 6 wafers
*Single wafer carrier
|style="background:WhiteSmoke; color:black"|
*Carrier for up to 6 wafers
|
*Vacuum-free edge-grip chucks for 50 mm, 100 mm & 150 mm, and 200 mm substrates
*Vacuum-free edge-grip chucks for 50 mm, 100 mm & 150 mm, and 200 mm substrates
*Chip chuck for chips & 2" substrates
*Chip chuck for chips & 50 mm substrates
|style="background:WhiteSmoke; color:black"|
|
*Vacuum-free edge-grip chuck for 100 mm & 150 mm substrates
*Vacuum-free edge-grip chuck for 100 mm & 150 mm substrates
*Chip chuck for chips & 2" substrates
*Chip chuck for chips & 50 mm substrates
|style="background:WhiteSmoke; color:black"|
| Vacuum chuck
Vacuum chuck
| Vacuum chuck
|style="background:WhiteSmoke; color:black"|
Vacuum chuck
|-
|-
 
! scope=row style="text-align: left;" | Process temperature
!style="background:silver; color:black" align="center" valign="center" rowspan="3"|Process parameters
| Room temperature
|style="background:LightGrey; color:black"|Temperature
| Room temperature
 
| Room temperature
|style="background:WhiteSmoke; color:black"|
| Room temperature
Room temperature
| Room temperature
|style="background:WhiteSmoke; color:black"|
| Room temperature
Room temperature
|style="background:WhiteSmoke; color:black"|
Room temperature
|style="background:WhiteSmoke; color:black"|
Room temperature
|style="background:WhiteSmoke; color:black"|
Room temperature
|-
|-
|style="background:LightGrey; color:black"|Agitation
! scope=row style="text-align: left;" | Process agitation
 
| No agitation allowed
|style="background:WhiteSmoke; color:black"|
| Magnetic stirrer
Magnetic stirrer
| Rotation
|style="background:WhiteSmoke; color:black"|
| Rotation
Rotation
| Rotation
|style="background:WhiteSmoke; color:black"|
| Rotation
Rotation
|style="background:WhiteSmoke; color:black"|
Rotation
|style="background:WhiteSmoke; color:black"|
Rotation
|-
|-
|style="background:LightGrey; color:black"|Rinse
! scope=row style="text-align: left;" | Process rinse
 
| Process dependent
|style="background:WhiteSmoke; color:black"|
| IPA
IPA
| IPA
|style="background:WhiteSmoke; color:black"|
| DI water
IPA
| DI water
|style="background:WhiteSmoke; color:black"|
| DI water
DI water
|style="background:WhiteSmoke; color:black"|
DI water
|style="background:WhiteSmoke; color:black"|
DI water
 
|-
|-
!style="background:silver; color:black" align="center" valign="center" rowspan="3"|Substrates
! scope=row style="text-align: left;" | Substrate size
|style="background:LightGrey; color:black"|Substrate size
|
 
* Chips
|style="background:WhiteSmoke; color:black"|
* 50 mm wafers
* 100 mm wafers
* 150 mm wafers
|
* Chips
* Chips
* 50 mm wafers
* 50 mm wafers
Line 148: Line 124:
* 150 mm wafers
* 150 mm wafers
* 200 mm wafers
* 200 mm wafers
|style="background:WhiteSmoke; color:black"|
|
* Chips (5mm to 2")
* Chips (5mm to 2")
* 50 mm wafers
* 50 mm wafers
Line 154: Line 130:
* 150 mm wafers
* 150 mm wafers
* 200 mm wafers
* 200 mm wafers
|style="background:WhiteSmoke; color:black"|
|
* Chips (5mm to 2")
* Chips (5mm to 50 mm)
* 100 mm wafers
* 100 mm wafers
* 150 mm wafers
* 150 mm wafers
|style="background:WhiteSmoke; color:black"|
|
* 100 mm wafers
* 100 mm wafers
* 150 mm wafers
* 150 mm wafers
* 200 mm wafers (may require tool change)
* 200 mm wafers (may require tool change)
|style="background:WhiteSmoke; color:black"|
|
* 100 mm wafers
* 100 mm wafers
* 150 mm wafers
* 150 mm wafers
* 200 mm wafers (may require tool change)
* 200 mm wafers (may require tool change)
|-
|-
|style="background:LightGrey; color:black"|Allowed materials
! scope=row style="text-align: left;" | Allowed materials
 
| All cleanroom approved materials
|style="background:WhiteSmoke; color:black"|
|
*Silicon and glass substrates
*Silicon and glass substrates
*Film or pattern of all but Type IV
*Film or pattern of all but Type IV
|style="background:WhiteSmoke; color:black"|
| All cleanroom approved materials
All cleanroom approved materials
|
|style="background:WhiteSmoke; color:black"|
*All cleanroom approved materials
*All cleanroom approved materials
*Film or pattern of all types
*Film or pattern of all types
|style="background:WhiteSmoke; color:black"|
|
*Silicon and glass substrates
*Silicon and glass substrates
*Film or pattern of all but Type IV
*Films, or patterned films, of any material except type IV (Pb, Te)
|style="background:WhiteSmoke; color:black"|
|
*Silicon, III-V, and glass substrates
*Silicon, III-V, and glass substrates
*Film or pattern of all but Type IV
*Films, or patterned films, of any material except type IV (Pb, Te)
|-
|-
|style="background:LightGrey; color:black"|Batch
! scope=row style="text-align: left;" | Batch size
 
| 1 - 5
|style="background:WhiteSmoke; color:black" align="center"|
| 1 - 6
1 - 6
| 1
|style="background:WhiteSmoke; color:black" align="center"|
| 1
1
| 1 - 25
|style="background:WhiteSmoke; color:black" align="center"|
| 1 - 25
1
|style="background:WhiteSmoke; color:black" align="center"|
1 - 25  
|style="background:WhiteSmoke; color:black" align="center"|
1 - 25
|-
|}
|}
<br clear="all" />
<!-- TARAN 2020-03-05
==Developer-1 and Developer-2==
[[Image:Developer1&2.jpg|300x300px|thumb|right|Developer-1 (right) and Developer-2 (left) are located in C-1]]
'''Feedback to this section''': '''[mailto:labadviser@nanolab.dtu.dk?Subject=Feed%20back%20from%20page%20http://labadviser.nanolab.dtu.dk/index.php/Specific_Process_Knowledge/Lithography/Development#Developer-1_and_Developer-2 click here]'''
===<span style="color:red">This equipment was decommissioned January 2017!</span>===
Developer-1 and Developer-2 are manual developer baths for submersion development of AZ 5214E and AZ 4562 resists in AZ 351B developer. The developer is mixed 1:5 in water by the user prior to development start, and the wafer cassette is agitated manually by the user during development. The development time is controlled manually by the user. After development, the substrates are rinsed with water in the bench.
'''The user APV, and contact information can be found in LabManager: [http://labmanager.dtu.dk/function.php?module=Machine&view=view&mach=62 Developer-1] [http://labmanager.dtu.dk/function.php?module=Machine&view=view&mach=63 Developer-2]'''
===Process information===
'''Standard development time using vigorous agitation:'''
'''AZ 5214E:'''
*1.5µm resist: 60 sec
*2.2µm resist: 70 sec
*4.2µm resist: 3 min
'''AZ 4562:'''
*10µm resist: 5 min
'''Standard development procedure:'''
*Before using one of developer baths, please check the "Litho4_Dev-7up-KOH" logbook to find out when they were last used. A fresh bath can be reused without problems.
*The main rule is a developer made yesterday must be changed.
*During development, agitate the substrates by moving the carrier up and down.
*Rinse substrates with water for 4-5 min. after development.
*Spin-dry substrates or dry with nitrogen gun after rinsing.
====Procedure for making a new developer====
1. Switch off the heater, and dump the old developer.
2. 800ml "Developer AZ 351B" is mixed with 4000ml water in a special container in the fume hood.
3. Fill the bath with the developer mixture, and heat it to 22°C before use.


=== Equipment performance and process related parameters ===
=Decommisioned tools=
<span style="color:red">Developer 1 & 2 were decommissioned 2017-01.</span>


{| border="2" cellspacing="0" cellpadding="2"
[[Specific Process Knowledge/Lithography/Development/1and2_developer|Information about decommissioned tool can be found here.]]


!style="background:silver; color:black;" align="center" width="60"|Purpose
|style="background:LightGrey; color:black"|
|style="background:WhiteSmoke; color:black" align="center"|
Development of
*AZ 5214E
*AZ 4562
|-
!style="background:silver; color:black;" align="center" width="60"|Developer
|style="background:LightGrey; color:black"|
|style="background:WhiteSmoke; color:black" align="center"|
AZ 351B diluted 1:5 in water


(NaOH and sodium borate salt)
<span style="color:red">Developer 6 inch was decommissioned 2019-12.</span>
|-
!style="background:silver; color:black" align="center" valign="center" rowspan="2"|Method
|style="background:LightGrey; color:black"|Development
|style="background:WhiteSmoke; color:black" align="center"|
Submersion
|-
|style="background:LightGrey; color:black"|Handling
|style="background:WhiteSmoke; color:black" align="center"|
Cassette
|-
!style="background:silver; color:black" align="center" valign="center" rowspan="3"|Process parameters
|style="background:LightGrey; color:black"|Temperature
|style="background:WhiteSmoke; color:black" align="center"|
22°C
|-
|style="background:LightGrey; color:black"|Agitation
|style="background:WhiteSmoke; color:black" align="center"|
Manual
|-
|style="background:LightGrey; color:black"|Rinse
|style="background:WhiteSmoke; color:black" align="center"|
DI water
|-
!style="background:silver; color:black" align="center" valign="center" rowspan="3"|Substrates
|style="background:LightGrey; color:black"|Substrate size
|style="background:WhiteSmoke; color:black" align="center"|
* 100 mm wafers
|-
| style="background:LightGrey; color:black"|Allowed materials
|style="background:WhiteSmoke; color:black" align="center"|
Silicon, glass, and polymer substrates
 
Film or pattern of all types
|-
|style="background:LightGrey; color:black"|Batch
|style="background:WhiteSmoke; color:black" align="center"|
1-8
|-
|}
 
<br clear="all" />
-->
 
<!-- TARAN 2020-03-05
==Developer-6inch==
 
[[image:6inchDeveloper.jpg|300x300px|right|thumb|The Developer: 6inch bench is located in E-4]]
 
'''Feedback to this section''': '''[mailto:labadviser@nanolab.dtu.dk?Subject=Feed%20back%20from%20page%20http://labadviser.nanolab.dtu.dk/index.php/Specific_Process_Knowledge/Lithography/Developers#Developer-6inch click here]'''
 
===<span style="color:red">This equipment will be decommissioned December 2019!</span>===
 
The Developer: 6inch bench is an automated developer bath for submersion development of AZ 5214E and AZ 4562 resists in AZ 351B developer. The developer is mixed 1:5 in water by the equipment prior to development start. The developer is circulated during development, and the wafer cassette may be agitated by a mechanical elevator. The development time is controlled manually by the user. After development, the substrates are rinsed with water in the bench.
 
'''The user manual, user APV, and contact information can be found in [http://labmanager.dtu.dk/function.php?module=Machine&view=view&mach=189 LabManager]'''
 
===Process information===
 
'''Standard development time:'''
 
'''AZ 5214E:'''
*1.5µm resist: 60 sec
*2.2µm resist: 70 sec
*4.2µm resist: 3 min
'''AZ 4562:'''
*10µm resist: 5 min
 
=== Equipment performance and process related parameters ===
 
{| border="2" cellspacing="0" cellpadding="2"
 
!style="background:silver; color:black;" align="center" width="60"|Purpose
|style="background:LightGrey; color:black"|
|style="background:WhiteSmoke; color:black" align="center"|
Development of
*AZ 5214E
*AZ 4562
|-
!style="background:silver; color:black;" align="center" width="60"|Developer
|style="background:LightGrey; color:black"|
|style="background:WhiteSmoke; color:black" align="center"|
AZ 351B diluted 1:5 in water
 
(NaOH and sodium borate salt)
|-
!style="background:silver; color:black" align="center" valign="center" rowspan="2"|Method
|style="background:LightGrey; color:black"|Development
|style="background:WhiteSmoke; color:black" align="center"|
Submersion
|-
|style="background:LightGrey; color:black"|Handling
|style="background:WhiteSmoke; color:black" align="center"|
Cassette
|-
!style="background:silver; color:black" align="center" valign="center" rowspan="3"|Process parameters
|style="background:LightGrey; color:black"|Temperature
|style="background:WhiteSmoke; color:black" align="center"|
22°C
|-
|style="background:LightGrey; color:black"|Agitation
|style="background:WhiteSmoke; color:black" align="center"|
Circulation and mechanical
|-
|style="background:LightGrey; color:black"|Rinse
|style="background:WhiteSmoke; color:black" align="center"|
DI water
|-
!style="background:silver; color:black" align="center" valign="center" rowspan="3"|Substrates
|style="background:LightGrey; color:black"|Substrate size
|style="background:WhiteSmoke; color:black" align="center"|
* 100 mm wafers
* 150 mm wafers
|-
| style="background:LightGrey; color:black"|Allowed materials
|style="background:WhiteSmoke; color:black" align="center"|
Silicon, glass, and polymer substrates
 
Film or pattern of all types
|-
|style="background:LightGrey; color:black"|Batch
|style="background:WhiteSmoke; color:black" align="center"|
1-25
|-
|}
 
<br clear="all" />
-->
 
==Manual beaker development in fumehood==
Beaker development is a fall-back option if you have a process, which is not compatible with the automatic, or semi-automatic, tools. We always recommend using, or at least trying, the automatic and semi-automatic tools, instead of using manual beaker development.
 
Manual beaker development is necessary for some processes, but should be avoided if possible, due to the fact that it is notoriously difficult to get a stable repeatable process - especially when multiple users are sharing the same process; everybody simply does things a bit different from each other, which leads to changes in the process outcome. Some processes have a very narrow process window, which makes them inherently sensitive to small changes in the development. The manual development also has a much greater chance of producing particles, both from the operator and the environment.
 
Finally the safety of the operator is at a significantly higher risk, since any manual handling of chemicals carries the risk of accidental spills with it. This is especially problematic if the developer is TMAH based, where direct skin exposure of >1% TMAH on a few percent of the body must be treated as a life-threatening event.
 
===Special rules for manual beaker development===
*Automatic agitation methods are not allowed - this includes magnetic stirring or sonication
*Manual agitation methods, which create large waves or turbulence in the development solution, are not allowed
*Users must submit a risk assessment for any process requiring manual beaker development
*Any users requiring manual beaker development of TMAH must provide valid reasons for not using the already available automatic and semi-automatic tools
 
===Standard manual beaker development procedure===
[[File:Beaker_development_v1.png|600px|thumb|Standard procedure for manual beaker development in fume hood:<br>1) Submerge exposed substrate into development solution<br>2) When timer ends, move substrate directly into Rinse 1<br>3) After a few seconds, move substrate into Rinse 2*<br>4) Remove developed substrate for drying<br>*It is allowed to omit the Rinse 2 step|right]]
The standard procedure for manual beaker development in a fume hood is as follows:
#Prepare development process
#Perform development
#Clean up
 
'''Prepare development process'''
*Write the chemical label, which must always be present in your chemical setup - your write your label <i>before</i> pouring the chemical
*Find the beakers required for your process
*Find the items required for holding/submerging your substrate during the process
*Find carriers or other storage units for placing your substrate after the process has finished
*Find a timer - make sure it works as you expect it to, before submerging your substrate into the development solution and discovering that the timer is in fact broken
*Get some cleanroom wipes and keep them nearby, for wiping any drops spilled during handling
*<span style="color:red">Do not cover too many of the exhaust holes in the fume hood table, as this will reduce the efficiency of the exhaust, which reduces safety</span>
*<span style="color:red">Do not place your beakers too close to the fume hood sash, as this can make it difficult to efficiently extract the fumes escaping from the beakers, which reduces safety</span>
 
'''Perform development'''
#Put on the appropriate personal protection gear
#Pour rinsing agent into Rinse 1 and Rinse 2 beakers - typically DI water or IPA
#Pour development solution into development beaker
#Place exposed substrate in the appropriate carrier
#Set timer
#Submerge substrate into development beaker
#Start timer immediately
#When timer is 5 seconds from ending, prepare to lift the substrate out of the development beaker
#Lift substrate out of development beaker - it can help to lift it at a slight angle, to allow liquids to drain more easily from large surfaces
#Submerge it immediately into Rinse 1
#Agitate up/down for at least a few seconds
#Move substrate into Rinse 2*
#Agitate slightly
#The developed substrate can now be removed and dried
 
<nowiki>*</nowiki>It is allowed to omit the Rinse 2 step
 
'''Clean up'''
*Pour Rinse 1 and Rinse 2 into appropriate waste: water goes into the sink, IPA goes into C-waste drain
*Rinse beakers with the DI-water gun
*Pour development solution into appropriate waste: solvent based developer goes into C-waste drain. <span style="color:red">NB! TMAH is an aqueous alkaline solution, which must never be mixed with solvents! TMAH waste goes into the dedicated TMAH waste container, stored in the chemical cabinet in E-4.</span>
*If your developer solution is not TMAH based:
**Rinse beaker 3 times, discard water into sink
*If your developer solution is TMAH based:
**Rinse beaker once with DI-water and discard this into the TMAH waste
**Rinse beaker two more times, discarding the water into the sink
*Hang all beakers to dry on the drying rack
*Erase the chemical label text
*Wipe any droplets on the fume hood surface
*Discard any napkins/other trash in the bin inside the fume hood
 
==Developer: SU8 (Wet Bench)==
[[Image:SU8dev.JPG|400px|right|thumb|The Developer: SU8 (Wet Bench) is located in E-4.]]
 
The SU8-Developer bench is a manually operated wet bench for submersion development of SU-8 photoresist in PGMEA (supplied in the cleanroom as mr-Dev 600). The development process is in two stages; one bath (FIRST) to dissolve the bulk of the resist, and a second, cleaner bath (FINAL) to finish the development. The development time is controlled manually by the user. After development, the substrates are rinsed with IPA in dedicated IPA bath and put for drying in the empty bath.
 
The user manual, user APV, and contact information can be found in [http://labmanager.dtu.dk/function.php?module=Machine&view=view&mach=509 LabManager: Developer: SU8(Wet Bench)] - '''requires login'''
 
===Process information===
Several aspects of the outcome of SU-8 processing are affected by the development process. The lithographic resolution is affected by the time between PEB (post-exposure bake) and development, as the cross-linking process continues in the interface between exposed and unexposed regions even at room temperature. Cracks in the structures is affected by two things; the development time, and how much has previously been developed in the developer bath. Cracking is worse with longer development time, and worst in a new developer bath. The effect of the developer use quickly saturates (5-10 wafers). Finally, the stability of fine structures (high aspect ratio) is affected by the rinse after development, as the lower surface tension of IPA compared to PGMEA reduces pattern collapse during drying.
 
 
Development time is strongly dependent on the SU-8 thickness.
*Minimum development time: 1 min per 20 µm in FIRST
 
 
Suggestions:
*2-5µm: 2 min. in FIRST; 2 min. in FINAL
*40µm: 5 min. in FIRST; 5 min. in FINAL (however, 3 min. in FIRST and 2 min. in FINAL is sufficient)
*180-250µm: 15 min. in FIRST; 15 min. in FINAL
 
=== Equipment performance and process related parameters ===
 
{|border="1" cellspacing="1" cellpadding="10" style="text-align:left;"
 
!style="background:silver; color:black;" align="center" width="60"|Purpose
|style="background:LightGrey; color:black"|
|style="background:WhiteSmoke; color:black"|
Development of:
*SU-8
|-
!style="background:silver; color:black;" align="center" width="60"|Developer
|style="background:LightGrey; color:black"|
|style="background:WhiteSmoke; color:black"|
mr-Dev 600
 
(PGMEA)
|-
!style="background:silver; color:black" align="center" valign="center" rowspan="2"|Method
|style="background:LightGrey; color:black"|Development
|style="background:WhiteSmoke; color:black"|
Submersion
|-
|style="background:LightGrey; color:black"|Handling
|style="background:WhiteSmoke; color:black"|
Single wafer holder
|-
!style="background:silver; color:black" align="center" valign="center" rowspan="3"|Process parameters
|style="background:LightGrey; color:black"|Temperature
|style="background:WhiteSmoke; color:black"|
Room temperature
|-
|style="background:LightGrey; color:black"|Agitation
|style="background:WhiteSmoke; color:black"|
Magnetic stirrer
|-
|style="background:LightGrey; color:black"|Rinse
|style="background:WhiteSmoke; color:black"|
IPA
|-
!style="background:silver; color:black" align="center" valign="center" rowspan="3"|Substrates
|style="background:LightGrey; color:black"|Substrate size
|style="background:WhiteSmoke; color:black"|
*100 mm wafers
*150 mm wafers, check the liquid level in the baths
*200 mm wafer, check the liquid level in the baths
|-
| style="background:LightGrey; color:black"|Allowed materials
|style="background:WhiteSmoke; color:black"|
*Silicon and glass substrates
*Film, or pattern, of all materials except Type IV
|-
|style="background:LightGrey; color:black"|Batch
|style="background:WhiteSmoke; color:black"|
1-6
|-
|}
 
<br clear="all" />
 
==Developer: E-beam 02==
[[Image:IMG 2464.JPG|400px|right|thumb|Developer: E-beam 02 is located in E-4.]]
 
Developer: E-beam 02 is a manually operated, single substrate puddle developer. It uses the ZED-N50 or AR 600-50 developers and IPA for rinsing. The substrates are loaded manually one by one into the developer. Developer dispense, puddle time, IPA rinse, and drying is then performed automatically by the equipment.
 
'''[https://www.youtube.com/watch?v=btinNzYnLnY Training video]''' (for Developer: TMAH Manual, but it is the same model)
 
The user manual, user APV, and contact information can be found in [http://labmanager.dtu.dk/function.php?module=Machine&view=view&mach=324 LabManager] - '''requires login'''
 
===Process information===
All recipes use the following structure:
#Pressurize the developer canister
#Dispense puddle while rotating substrate slowly
#Puddle development while not rotating
#Agitate substrate once per 15 seconds by rotating slowly for 1 second
#Spin off developer
#Clean substrate with IPA
#Dry substrate and chamber with nitrogen
 
Multi-puddle recipes repeat steps 2-5 for the given number of puddles.
 
 
'''Process recipes'''<br>
N50 recipes have the letter "N" in them. AR-600-50 recipes have the letter "A"  in them. The number is the development time in seconds:
*01 Rinse
*02 N 15
*03 N 30
*04 N 60
*05 N 90
*06 N 120
*07 N 180
*08 N 300
*09 N 600
*10 N 2x60
*11 N 5x60
*12 A 15
*13 A 30
*14 A 60
*15 A 90
*16 A 120
*17 A 180
*18 A 300
*19 A 600
*20 A 2x60
*21 A 5x60
 
=== Equipment performance and process related parameters ===
 
{|border="1" cellspacing="1" cellpadding="10" style="text-align:left;"
 
|-
!style="background:silver; color:black;" align="center" width="60"|Purpose
|style="background:LightGrey; color:black"|
|style="background:WhiteSmoke; color:black"|
Development of:
*CSAR
*ZEP520A
 
|-
!style="background:silver; color:black;" width="60"|Developer
|style="background:LightGrey; color:black"|
|style="background:WhiteSmoke; color:black"|
*AR 600-50
*ZED N-50
|-
!style="background:silver; color:black" align="center" valign="center" rowspan="2"|Method
|style="background:LightGrey; color:black"|Development
|style="background:WhiteSmoke; color:black"|
Puddle
|-
|style="background:LightGrey; color:black"|Handling
|style="background:WhiteSmoke; color:black"|
*Chip chuck for chips
*Non-vacuum chuck for 2" wafers
*Non-vacuum chuck for 100 mm and 150 mm wafers
*Non-vacuum chuck for 200 mm wafers
|-
!style="background:silver; color:black" align="center" valign="center" rowspan="3"|Process parameters
|style="background:LightGrey; color:black"|Temperature
|style="background:WhiteSmoke; color:black"|
Room temperature
|-
|style="background:LightGrey; color:black"|Agitation
|style="background:WhiteSmoke; color:black"|
1 second rotational agitation at 30 rpm every 15 seconds
|-
|style="background:LightGrey; color:black"|Rinse
|style="background:WhiteSmoke; color:black"|
IPA
|-
!style="background:silver; color:black" align="center" valign="center" rowspan="3"|Substrates
|style="background:LightGrey; color:black"|Substrate size
|style="background:WhiteSmoke; color:black"|
*Chips
*2" wafers
*100 mm wafers
*150 mm wafers
*200 mm wafers
|-
| style="background:LightGrey; color:black"|Allowed materials
|style="background:WhiteSmoke; color:black"|
*All cleanroom approved materials
*Film, or pattern, of all materials except Type IV
|-
|style="background:LightGrey; color:black"|Batch size
|style="background:WhiteSmoke; color:black"|
1
|-
|}
 
<br clear="all" />
 
==Developer: TMAH Manual 02==
[[Image:IMG 2464.JPG|400px|right|thumb|Developer: TMAH Manual 02 is located in E-4.]]
 
Developer: TMAH Manual 02 is a manually operated, single substrate or chip puddle developer. It uses the TMAH based AZ 726 MIF developer (2.38 % TMAH in  water with a small amount of wetting agent). The substrates or chips are loaded manually one by one into the developer. Developer dispense, puddle time, water rinse, and drying is performed automatically by the equipment.
 
 
'''[https://www.youtube.com/watch?v=btinNzYnLnY Training video]'''
 
 
The user manual, user APV, and contact information can be found in [http://labmanager.dtu.dk/function.php?module=Machine&view=view&mach=324 LabManager] - '''requires login'''
 
===Process information===
All recipes use the following structure:
#Pressurize the TMAH canister
#Dispense puddle while rotating substrate slowly
#Puddle development while not rotating
#Agitate substrate once per 15 seconds by rotating slowly for 1 second
#Spin off developer
#Clean substrate and chamber with DI water
#Dry substrate and chamber with nitrogen
 
Multi-puddle recipes repeat steps 2-5 for the given number of puddles.
 
 
'''Process recipes'''<br>
SP: Single-puddle<br>
MP: Multi-puddle
 
*01 Rinse
*02 SP 15
*03 SP 30
*04 SP 60
*05 SP 90
*06 SP 120
*07 SP 300
*08 MP 2x60
*09 MP 5x60
*91 SP test
*92 MP test
 
=== Equipment performance and process related parameters ===
 
{|border="1" cellspacing="1" cellpadding="10" style="text-align:left;"
 
 
!style="background:silver; color:black;" align="center" width="60"|Purpose
|style="background:LightGrey; color:black"|
|style="background:WhiteSmoke; color:black"|
Development of UV resists:
*AZ nLOF
*AZ MiR 701
*AZ 5214E
*AZ 4562
Development of DUV resists:
*KRF M230Y
*KRF M35G
|-
!style="background:silver; color:black;" align="center" width="60"|Developer
|style="background:LightGrey; color:black"|
|style="background:WhiteSmoke; color:black"|
AZ 726 MIF<br>
(2.38% TMAH in water)
|-
!style="background:silver; color:black" align="center" valign="center" rowspan="2"|Method
|style="background:LightGrey; color:black"|Development
|style="background:WhiteSmoke; color:black"|
Puddle
|-
|style="background:LightGrey; color:black"|Handling
|style="background:WhiteSmoke; color:black"|
*Chip chuck for chips and 2" wafers
*Non-vacuum chuck for 100 mm and 150 mm wafers
|-
!style="background:silver; color:black" align="center" valign="center" rowspan="3"|Process parameters
|style="background:LightGrey; color:black"|Temperature
|style="background:WhiteSmoke; color:black"|
Room temperature
|-
|style="background:LightGrey; color:black"|Agitation
|style="background:WhiteSmoke; color:black"|
1 second rotational agitation at 30 rpm every 15 seconds
|-
|style="background:LightGrey; color:black"|Rinse
|style="background:WhiteSmoke; color:black"|
DI water
|-
!style="background:silver; color:black" align="center" valign="center" rowspan="3"|Substrates
|style="background:LightGrey; color:black"|Substrate size
|style="background:WhiteSmoke; color:black"|
*Chips (6-60 mm)
*100 mm wafers
*150 mm wafers
|-
| style="background:LightGrey; color:black"|Allowed materials
|style="background:WhiteSmoke; color:black"|
*All cleanroom approved materials
*Film, or pattern, of all materials except Type IV
|-
|style="background:LightGrey; color:black"|Batch size
|style="background:WhiteSmoke; color:black"|
1
|-
|}
<br clear="all" />
 
==Developer TMAH UV-lithography==
 
[[Image:SUSS DEV.JPG|400px|right|thumb|Developer: TMAH UV-lithography is located in E-4.]]
 
Developer TMAH UV-lithography was released Q4 2014.
 
Link to information about [[Specific_Process_Knowledge/Pattern_Design#Helpful_information_for_chip_layout|developer chuck size and hotplate pin positions]].
 
'''[https://www.youtube.com/watch?v=fs9DRH0Eo3k Training video]'''
 
 
The user manual, user APV, and contact information can be found in [http://labmanager.dtu.dk/function.php?module=Machine&view=view&mach=329 LabManager] - '''requires login'''
 
===[[Specific Process Knowledge/Lithography/Development/Developer TMAH UV-lithography processing|Process Information]]===
*[[Specific Process Knowledge/Lithography/Development/Developer_TMAH_UV-lithography_processing#General_Process_Information|General process information]]
*[[Specific Process Knowledge/Lithography/Development/Developer TMAH UV-lithography_processing#Process recommendations|Process recommendations]]
*[[Specific Process Knowledge/Lithography/Development/Developer TMAH UV-lithography processing#Standard Processes|Standard processes]]
 
=== Equipment performance and process related parameters ===
 
{|border="1" cellspacing="1" cellpadding="10" style="text-align:left;"
 
!style="background:silver; color:black;" width="60"|Purpose
|style="background:LightGrey; color:black"|
|style="background:WhiteSmoke; color:black"|
Development of
*AZ nLOF
*AZ MiR 701
*AZ 5214E
*AZ 4562
*DUV resists
|-
!style="background:silver; color:black;" width="60"|Developer
|style="background:LightGrey; color:black"|
|style="background:WhiteSmoke; color:black" |
AZ 726 MIF
 
(2.38% TMAH in water)
|-
!style="background:silver; color:black" align="center" valign="center" rowspan="2"|Method
|style="background:LightGrey; color:black"|Development
|style="background:WhiteSmoke; color:black"|
Puddle
|-
|style="background:LightGrey; color:black"|Handling
|style="background:WhiteSmoke; color:black"|
Vacuum chuck
|-
!style="background:silver; color:black" align="center" valign="center" rowspan="3"|Process parameters
|style="background:LightGrey; color:black"|Temperature
|style="background:WhiteSmoke; color:black"|
Room temperature
|-
|style="background:LightGrey; color:black"|Agitation
|style="background:WhiteSmoke; color:black"|
Rotation
|-
|style="background:LightGrey; color:black"|Rinse
|style="background:WhiteSmoke; color:black"|
DI water
|-
!style="background:silver; color:black" align="center" valign="center" rowspan="3"|Substrates
|style="background:LightGrey; color:black"|Substrate size
|style="background:WhiteSmoke; color:black"|
* 100 mm wafers
* 150 mm wafers
|-
| style="background:LightGrey; color:black"|Allowed materials
|style="background:WhiteSmoke; color:black"|
Silicon and glass substrates
 
Film or pattern of all except Type IV
|-
|style="background:LightGrey; color:black"|Batch
|style="background:WhiteSmoke; color:black"|
1-25
|-
|}
<br clear="all" />


{{:Specific Process Knowledge/Lithography/Development/DUV_developer}}
[[Specific Process Knowledge/Lithography/Development/6inch_developer|Information about decommissioned tool can be found here.]]